Method for recovering iron phosphate in iron phosphate production filtrate

By adjusting the pH value of the iron phosphate filtrate and adding cationic polyacrylamide for flocculation and precipitation, combined with the treatment of ferrous sulfate and hydrochloric acid, the yield of iron phosphate and product purity were successfully improved, and the difficulty in collecting in iron phosphate production was solved The problem has improved the efficiency of the enterprise.

CN118894508APending Publication Date: 2024-11-05ANHUI JIETU NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410930094.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

During the iron phosphate production process, the filtered iron phosphate is difficult to be effectively collected, resulting in a decrease in yield and the existing flocculants are difficult to use, affecting product quality.

Method used

By adjusting the pH value of the iron phosphate filtrate to no more than 2, and adding cationic polyacrylamide for flocculation and precipitation, after separation and precipitation, add a mixed solution of ferrous sulfate and hydrochloric acid for reaction, remove the residue of cationic polyacrylamide, and finally pass through multiple Sub-washing and drying sintering to give anhydrous iron phosphate.

Benefits of technology

It improves the yield of iron phosphate, reduces resource waste, ensures the purity and quality of the product, and enhances the efficiency of the enterprise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004939371910000091
    Figure BDA0004939371910000091
  • Figure BDA0004939371910000101
    Figure BDA0004939371910000101
Patent Text Reader

Abstract

The invention relates to a method for recovering iron phosphate in iron phosphate production filtrate, and belongs to the technical field of iron phosphate wastewater treatment. The invention relates to a method for recovering iron phosphate in iron phosphate production filtrate, which comprises the following steps: adjusting the pH value of the iron phosphate filtrate to be not more than 2, adding cationic polyacrylamide for precipitation, and separating the precipitate to obtain the iron phosphate. The device can efficiently collect iron phosphate entering wastewater through filtration in iron phosphate production, effectively improve the yield of iron phosphate, improve the benefits of enterprises and reduce the waste of resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of iron phosphate wastewater treatment, and in particular to a method for recovering iron phosphate in an iron phosphate production filtrate. Background Art

[0002] The characteristics of lithium iron phosphate batteries are large discharge capacity, low price, wide material sources, non-toxicity, and no environmental pollution. With the development of technologies and markets such as energy storage (wind energy, solar energy), 5G, and new energy vehicles, the demand for batteries is increasing, especially the safety of lithium iron phosphate batteries. Lithium iron phosphate batteries are most likely to become the most widely used electric vehicle batteries in the future. As a precursor of lithium iron phosphate, the demand for iron phosphate is also increasing.

[0003] During the production of iron phosphate, a small amount of iron phosphate will filter into the wastewater after filtration and cannot be collected, resulting in a decrease in the yield of iron phosphate. At the same time, the acidic pH of iron phosphate wastewater is low and the salinity is high. Usually, flocculants are difficult to use, and it is difficult to collect iron phosphate in the wastewater. In addition, flocculants are prone to produce a large amount of residues, which affects the quality of iron phosphate and is not used. The production of iron phosphate requires a large amount of water, so although the iron phosphate content in the wastewater is low, it can be collected efficiently and is considerable, which can effectively improve the product yield, improve the efficiency of the enterprise and reduce the waste of resources. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the embodiments of the present application includes providing a method for recovering iron phosphate in the filtrate of iron phosphate production. The iron phosphate that filters into the wastewater during the production of iron phosphate can be efficiently collected, the yield of iron phosphate can be effectively improved, the benefits of the enterprise can be improved, and the waste of resources can be reduced.

[0005] In a first aspect, an embodiment of the present application provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising: adjusting the pH value of the iron phosphate filtrate to no more than 2, adding cationic polyacrylamide for precipitation, and separating the precipitate to obtain iron phosphate.

[0006] The present application adjusts the pH value of the iron phosphate filtrate to no more than 2, which is beneficial to the subsequent use of a flocculant to flocculate and precipitate the iron phosphate in the filtrate, and avoids the reaction between the iron ions and the phosphate ions in the filtrate to generate new iron phosphate precipitates without a crystalline structure; cationic polyacrylamide is then added to flocculate and precipitate the iron phosphate in the filtrate, so as to collect the iron phosphate with a crystalline structure that filters into the wastewater during the production of iron phosphate, thereby effectively improving the yield of the iron phosphate product, improving the efficiency of the enterprise and reducing the waste of resources.

[0007] In some embodiments of the present application, the method for separating the precipitate includes: adding a mixed solution of ferrous sulfate and hydrochloric acid to the precipitate for reaction.

[0008] The present application adds a mixed solution of ferrous sulfate and hydrochloric acid to the precipitate, thereby destroying the molecular structure of the cationic polyacrylamide so that it can be dissolved in the liquid, thereby preventing the cationic polyacrylamide from generating a large amount of residues that affect the quality of the ferric phosphate.

[0009] In some embodiments of the present application, the process further comprises: adding water to the precipitate after the reaction to wash it multiple times.

[0010] The present application then washes the precipitate with water for multiple times to remove ferrous ions, so as to obtain relatively pure ferric phosphate.

[0011] In some embodiments of the present application, the washing is terminated when: the ferrous ion content in the last washing solution is less than 0.1 mg / L or the conductivity of the last washing solution is less than 10 μS / cm.

[0012] In the present application, the washing of the precipitate can be stopped until the ferrous ion content is less than a certain value or the conductivity is less than a certain value, and relatively pure ferric phosphate can be obtained.

[0013] In some embodiments of the present application, the separated precipitated iron phosphate is dried and sintered to obtain anhydrous iron phosphate.

[0014] The precipitated iron phosphate separated in the present application is iron phosphate dihydrate, and anhydrous iron phosphate product is obtained through drying and sintering.

[0015] In some embodiments of the present application, the amount of cationic polyacrylamide added is 10-30 mg / L.

[0016] The present application adds a suitable amount of cationic polyacrylamide to the filtrate, so as to efficiently flocculate and precipitate the iron phosphate in the filtrate.

[0017] In some embodiments of the present application, the pH of the ferric phosphate filtrate is adjusted to 1.5-1.8.

[0018] The present application adjusts the pH value of the iron phosphate filtrate to an appropriate range, which can not only facilitate the subsequent use of a flocculant to flocculate and precipitate the iron phosphate in the filtrate, but also avoid the reaction between iron ions and phosphate ions in the filtrate to generate new iron phosphate precipitates without a crystalline structure, and collect the iron phosphate with a crystalline structure that filters into the wastewater during the iron phosphate production by flocculation precipitation.

[0019] In some embodiments of the present application, the mass ratio of the precipitate to the mixed solution of ferrous sulfate and hydrochloric acid is 1:3-5.

[0020] The present application adds a suitable amount of a mixed solution of ferrous sulfate and hydrochloric acid to the precipitate for reaction, which can effectively remove the cationic polyacrylamide and avoid the cationic polyacrylamide from producing a large amount of residues that affect the quality of the ferric phosphate.

[0021] In some embodiments of the present application, the pH value of the mixed solution of ferrous sulfate and hydrochloric acid is 1.8-2.0.

[0022] In the present application, the mixed solution of ferrous sulfate and hydrochloric acid is adjusted to a suitable pH value and reacted with a precipitate, which can facilitate the decomposition and removal of cationic polyacrylamide and avoid the generation of a large amount of cationic polyacrylamide residues that affect the quality of iron phosphate.

[0023] In some embodiments of the present application, the concentration of ferrous ions in the mixed solution of ferrous sulfate and hydrochloric acid is 20-100 mg / L.

[0024] The present application uses a mixed solution of ferrous sulfate and hydrochloric acid for precipitation reaction to ensure a certain concentration of ferrous ions, which can react with cationic polyacrylamide efficiently to remove cationic polyacrylamide. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0026] The embodiment of the present application provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising: adjusting the pH value of the iron phosphate filtrate to no more than 2, adding cationic polyacrylamide for precipitation, and separating the precipitate to obtain iron phosphate.

[0027] The present application adjusts the pH value of the iron phosphate filtrate to no more than 2, which is beneficial to the subsequent use of a flocculant to flocculate and precipitate the iron phosphate in the filtrate, and avoids the reaction between the iron ions and the phosphate ions in the filtrate to generate new iron phosphate precipitates without a crystalline structure; cationic polyacrylamide is then added to flocculate and precipitate the iron phosphate in the filtrate, so as to collect the iron phosphate with a crystalline structure that filters into the wastewater during the production of iron phosphate, thereby effectively improving the yield of the iron phosphate product, improving the efficiency of the enterprise and reducing the waste of resources.

[0028] In some embodiments of the present application, aqueous ammonia may be added to the ferric phosphate filtrate to adjust the pH value, but is not limited to.

[0029] In some embodiments of the present application, after adding cationic polyacrylamide to the ferric phosphate filtrate, stirring at 100-200r / min for 10-20min for precipitation. As an example, the stirring speed may be, but is not limited to, 100r / min, 120r / min, 140r / min, 150r / min, 160r / min, 180r / min, 200r / min. The stirring time may be, but is not limited to, 10min, 12min, 14min, 15min, 16min, 18min, 20min.

[0030] In some embodiments of the present application, the method for separating the precipitate includes: adding a mixed solution of ferrous sulfate and hydrochloric acid to the precipitate for reaction. Adding the mixed solution of ferrous sulfate and hydrochloric acid to the precipitate can destroy the molecular structure of the cationic polyacrylamide so that it can be dissolved in the liquid, thereby preventing the cationic polyacrylamide from generating a large amount of residues that affect the quality of the ferric phosphate.

[0031] In some embodiments of the present application, after a mixed solution of ferrous sulfate and hydrochloric acid is added to the precipitate for reaction, centrifugation is performed at 700-900 r / min. As an example, the centrifugal speed may be, but is not limited to, 700 r / min, 750 r / min, 800 r / min, 850 r / min, and 900 r / min.

[0032] In some embodiments of the present application, the method further comprises: adding water to the precipitate after the reaction to wash it multiple times. The precipitate is washed multiple times with water to remove ferrous ions, so as to obtain relatively pure ferric phosphate.

[0033] In some embodiments of the present application, the washing is terminated when the ferrous ion content in the last washing solution is less than 0.1 mg / L or the conductivity of the last washing solution is less than 10 μs / cm. Washing the precipitate can be stopped when the ferrous ion content is less than a certain value or the conductivity is less than a certain value, and relatively pure iron phosphate can be obtained.

[0034] In some embodiments of the present application, the separated precipitated iron phosphate is dried and sintered to obtain anhydrous iron phosphate. The separated precipitated iron phosphate is dihydrate iron phosphate, which is dried and sintered to obtain anhydrous iron phosphate product.

[0035] In some embodiments of the present application, the addition amount of cationic polyacrylamide is 10-30 mg / L. Adding a suitable amount of cationic polyacrylamide to the filtrate can more efficiently collect the ferric phosphate in the filtrate by flocculation precipitation. As an example, the addition amount of cationic polyacrylamide can be, but is not limited to, 10 mg / L, 12 mg / L, 15 mg / L, 16 mg / L, 18 mg / L, 20 mg / L, 22 mg / L, 25 mg / L, 26 mg / L, 28 mg / L, 30 mg / L.

[0036] In some embodiments of the present application, the pH of the ferric phosphate filtrate is adjusted to 1.5-1.8. Adjusting the pH value of the ferric phosphate filtrate to an appropriate range can not only facilitate the subsequent use of a flocculant to flocculate and precipitate the ferric phosphate in the filtrate, but also avoid the reaction of iron ions and phosphate ions in the filtrate to generate new ferric phosphate precipitates without a crystalline structure, and collect the ferric phosphate with a crystalline structure that filters into the wastewater during the production of ferric phosphate by flocculation and precipitation.

[0037] In some embodiments of the present application, the mass ratio of the precipitate to the mixed solution of ferrous sulfate and hydrochloric acid is 1:3-5. Adding a suitable amount of the mixed solution of ferrous sulfate and hydrochloric acid to the precipitate for reaction can efficiently remove the cationic polyacrylamide and avoid the cationic polyacrylamide from producing a large amount of residues that affect the quality of ferric phosphate. As an example, the mass ratio of the precipitate to the mixed solution of ferrous sulfate and hydrochloric acid can be, but is not limited to, 1:3, 1:4, 1:5.

[0038] In some embodiments of the present application, the pH value of the mixed solution of ferrous sulfate and hydrochloric acid is 1.8-2.0. The mixed solution of ferrous sulfate and hydrochloric acid is adjusted to a suitable pH value and reacted with a precipitate to facilitate the decomposition and removal of cationic polyacrylamide, thereby preventing the cationic polyacrylamide from producing a large amount of residues that affect the quality of ferric phosphate.

[0039] In some embodiments of the present application, the concentration of ferrous ions in the mixed solution of ferrous sulfate and hydrochloric acid is 20-100mg / L. Ferrous ions in the mixed solution of ferrous sulfate and hydrochloric acid with precipitation reaction ensure a certain concentration, and can efficiently react with cationic polyacrylamide to remove cationic polyacrylamide. As an example, the concentration of ferrous ions in the mixed solution of ferrous sulfate and hydrochloric acid can be but not limited to 20mg / L, 30mg / L, 40mg / L, 50mg / L, 60mg / L, 70mg / L, 80mg / L, 90mg / L, 100mg / L.

[0040] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0041] Example 1

[0042] This embodiment provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising:

[0043] (1) adding 30% ammonia water to the ferric phosphate filtrate to adjust the pH value to 1.5, then adding 10 mg / L cationic polyacrylamide, and stirring at 200 r / min for 10 min to precipitate;

[0044] (2) placing the liquid in step (1) into a sedimentation tank for 30 minutes of sedimentation, discharging the supernatant, and injecting the sludge into a press through a diaphragm pump for pressure filtration and dehydration to obtain a filter cake;

[0045] (3) placing the filter cake obtained by filter pressing and dehydration into a stirring tank, adding a mixed solution of ferrous sulfate and hydrochloric acid and stirring evenly, adjusting the pH of the mixed solution of ferrous sulfate and hydrochloric acid to 1.8, the mass ratio of the filter cake to the mixed solution of ferrous sulfate and hydrochloric acid to 1:3, and the ferrous ion concentration to 20 mg / L;

[0046] (4) centrifuging the mixed solution in the stirring tank, discharging the supernatant, adding water to wash the mixture several times, and repeating the washing until the conductivity of the washing solution is less than 10 μS / cm;

[0047] (5) The washed precipitate in step (4) is taken out, the supernatant is discharged, the precipitate is placed in an oven for drying and dehydration at 100° C., and then the dried ferric phosphate is placed in a muffle furnace for sintering at 600° C. to obtain an anhydrous ferric phosphate product.

[0048] Example 2

[0049] This embodiment provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising:

[0050] (1) adding 30% ammonia water to the ferric phosphate filtrate to adjust the pH value to 1.8, then adding 30 mg / L cationic polyacrylamide, stirring and mixing at 150 r / min for 15 min to precipitate;

[0051] (2) placing the liquid in step (1) into a sedimentation tank for 30 minutes of sedimentation, discharging the supernatant, and injecting the sludge into a press through a diaphragm pump for pressure filtration and dehydration to obtain a filter cake;

[0052] (3) placing the filter cake obtained by filter pressing and dehydration into a stirring tank, adding a mixed solution of ferrous sulfate and hydrochloric acid and stirring evenly, the pH of the mixed solution of ferrous sulfate and hydrochloric acid is adjusted to 1.9, the mass ratio of the filter cake to the mixed solution of ferrous sulfate and hydrochloric acid is 1:5, and the ferrous ion concentration is 100 mg / L;

[0053] (4) centrifuging the mixed solution in the stirring tank, discharging the supernatant, adding water to wash the mixture several times, and repeating the washing until the conductivity of the washing solution is less than 10 μS / cm;

[0054] (5) The washed precipitate in step (4) is taken out, the supernatant is discharged, the precipitate is placed in an oven for drying and dehydration at 100° C., and then the dried ferric phosphate is placed in a muffle furnace for sintering at 600° C. to obtain an anhydrous ferric phosphate product.

[0055] Example 3

[0056] This embodiment provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising:

[0057] (1) adding 30% ammonia water to the ferric phosphate filtrate to adjust the pH value to 1.6, then adding 20 mg / L cationic polyacrylamide, stirring and mixing at 100 r / min for 20 min to precipitate;

[0058] (2) placing the liquid in step (1) into a sedimentation tank for 30 minutes of sedimentation, discharging the supernatant, and injecting the sludge into a press through a diaphragm pump for pressure filtration and dehydration to obtain a filter cake;

[0059] (3) placing the filter cake obtained by filter pressing and dehydration into a stirring tank, adding a mixed solution of ferrous sulfate and hydrochloric acid and stirring evenly, adjusting the pH of the mixed solution of ferrous sulfate and hydrochloric acid to 2.0, the mass ratio of the filter cake to the mixed solution of ferrous sulfate and hydrochloric acid to 1:4, and the ferrous ion concentration to 60 mg / L;

[0060] (4) centrifuging the mixed solution in the stirring tank, discharging the supernatant, adding water to wash the mixture several times, and repeating the washing until the conductivity of the washing solution is less than 10 μS / cm;

[0061] (5) The washed precipitate in step (4) is taken out, the supernatant is discharged, the precipitate is placed in an oven for drying and dehydration at 100° C., and then the dried ferric phosphate is placed in a muffle furnace for sintering at 600° C. to obtain an anhydrous ferric phosphate product.

[0062] Comparative Example 1

[0063] This comparative example provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising:

[0064] (1) adding 30% ammonia water to the ferric phosphate filtrate to adjust the pH value to 2.5, then adding 10 mg / L cationic polyacrylamide, stirring and mixing at 200 r / min for 10 min to precipitate;

[0065] (2) placing the liquid in step (1) into a sedimentation tank for 30 minutes of sedimentation, discharging the supernatant, and injecting the sludge into a press through a diaphragm pump for pressure filtration and dehydration to obtain a filter cake;

[0066] (3) placing the filter cake obtained by filter pressing and dehydration into a stirring tank, adding a mixed solution of ferrous sulfate and hydrochloric acid and stirring evenly, adjusting the pH of the mixed solution of ferrous sulfate and hydrochloric acid to 1.8, the mass ratio of the filter cake to the mixed solution of ferrous sulfate and hydrochloric acid to 1:3, and the ferrous ion concentration to 20 mg / L;

[0067] (4) centrifuging the mixed solution in the stirring tank, draining the supernatant, adding water to wash the mixture several times, and repeating the washing until the ferrous ion content in the washing solution is less than 0.1 mg / L or the conductivity of the washing solution is less than 10 μS / cm;

[0068] (5) The washed precipitate in step (4) is taken out, the supernatant is discharged, the precipitate is placed in an oven for drying and dehydration at 100° C., and then the dried ferric phosphate is placed in a muffle furnace for sintering at 600° C. to obtain an anhydrous ferric phosphate product.

[0069] Comparative Example 2

[0070] This comparative example provides a method for recovering iron phosphate in an iron phosphate production filtrate, comprising:

[0071] (1) adding 30% ammonia water to the ferric phosphate filtrate to adjust the pH value to 1.5, then adding 10 mg / L anionic polyacrylamide, and stirring at 200 r / min for 10 min to precipitate;

[0072] (2) placing the liquid in step (1) into a sedimentation tank for 30 minutes of sedimentation, discharging the supernatant, and injecting the sludge into a press through a diaphragm pump for pressure filtration and dehydration to obtain a filter cake;

[0073] (3) placing the filter cake obtained by filter pressing and dehydration into a stirring tank, adding a mixed solution of ferrous sulfate and hydrochloric acid and stirring evenly, adjusting the pH of the mixed solution of ferrous sulfate and hydrochloric acid to 1.8, the mass ratio of the filter cake to the mixed solution of ferrous sulfate and hydrochloric acid to 1:3, and the ferrous ion concentration to 20 mg / L;

[0074] (4) centrifuging the mixed solution in the stirring tank, draining the supernatant, adding water to wash the mixture several times, and repeating the washing until the ferrous ion content in the washing solution is less than 0.1 mg / L or the conductivity of the washing solution is less than 10 μS / cm;

[0075] (5) The washed precipitate in step (4) is taken out, the supernatant is discharged, the precipitate is placed in an oven for drying and dehydration at 100° C., and then the dried ferric phosphate is placed in a muffle furnace for sintering at 600° C. to obtain an anhydrous ferric phosphate product.

[0076] Table 1 Recovery methods of Examples 1-3 and Comparative Examples 1-2

[0077] pH value of iron phosphate filtrate Flocculants Example 1 1.5 Cationic polyacrylamide Example 2 1.8 Cationic polyacrylamide Example 3 1.6 Cationic polyacrylamide Comparative Example 1 2.5 Cationic polyacrylamide Comparative Example 2 1.5 Anionic polyacrylamide

[0078] Test Example 1

[0079] The components of the iron phosphate recovered in Example 1-3 and Comparative Example 1-2 and the iron phosphate products produced by the iron phosphate production line were analyzed, and the results are shown in Table 2. The recovery rate of each iron phosphate was calculated, and the results are shown in Table 3.

[0080] Table 2 Iron phosphate composition

[0081]

[0082]

[0083] As can be seen from the results in Table 2, the Fe content, P content and Fe / P value of the iron phosphate recovered in Examples 1-3 and Comparative Example 2 are close to those of the iron phosphate product, indicating that the iron phosphate recovered in Examples 1-3 and Comparative Example 2 is the iron phosphate product with a crystalline structure that is filtered into the wastewater during the production of iron phosphate. This is because in Examples 1-3 and Comparative Example 2, the pH value of the iron phosphate filtrate is adjusted to be no more than 2, which avoids the reaction of iron ions and phosphate ions in the filtrate to generate new iron phosphate precipitates without a crystalline structure, thereby collecting the iron phosphate product with a crystalline structure that is filtered into the wastewater during the production of iron phosphate.

[0084] Table 3 Iron phosphate recovery

[0085] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Recovery rate (%) 99.8 99.9 99.8 680.2 71.1

[0086] As can be seen from the results in Table 3, the recovery rate of iron phosphate in Comparative Example 1 is too high because the pH value of the iron phosphate filtrate is adjusted to 2.5 in Comparative Example 1, so that the iron ions and phosphate ions in the filtrate generate a large amount of amorphous iron phosphate, which is manifested as an excessively high recovery rate. However, it is not the iron phosphate with a crystalline structure that penetrates into the wastewater during the iron phosphate production that is recovered by the present application, and has no product value. The recovery rate of iron phosphate in Comparative Example 2 is relatively low because the pH value of the iron phosphate filtrate is adjusted to no more than 2. Under this condition, the anionic polyacrylamide flocculation effect is poor and the recovery rate is low.

[0087] Test Example 2

[0088] In this test example, the bulk density of the iron phosphate dihydrate recovered from Example 1-3 and Comparative Example 1-2 and not sintered in a muffle furnace was tested. The results are shown in Table 4.

[0089] Table 4 Bulk density of recovered ferric phosphate

[0090] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 <![CDATA[Bulk density (g / cm 3 )]]> 0.891 0.899 0.881 0.522 0.883

[0091] It can be seen from the results in Table 4 that the loose density of the iron phosphate recovered in Comparative Example 1 is lower because the pH value of the iron phosphate filtrate in Comparative Example 1 is adjusted to 2.5, so that the iron ions and phosphate ions in the filtrate generate a large amount of amorphous iron phosphate, resulting in a lower loose density.

[0092] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A method for recovering iron phosphate from an iron phosphate production filtrate, characterized in that: include: The pH value of the ferric phosphate filtrate is adjusted to be no greater than 2, and then cationic polyacrylamide is added for precipitation, and the precipitate is separated to obtain ferric phosphate.

2. The method for recovering iron phosphate according to claim 1, characterized in that: The method for separating the precipitate comprises: adding a mixed solution of ferrous sulfate and hydrochloric acid to the precipitate for reaction.

3. The method for recovering iron phosphate according to claim 2, characterized in that: Also includes: Water is added to the precipitate after the reaction to wash it several times.

4. The method for recovering iron phosphate according to claim 3, characterized in that: The washing is terminated when the ferrous ion content in the last washing solution is less than 0.1 mg / L or the conductivity of the last washing solution is less than 10 μS / cm.

5. The method for recovering iron phosphate according to any one of claims 1 to 4, characterized in that: The separated precipitated iron phosphate is dried and sintered to obtain anhydrous iron phosphate.

6. The method for recovering iron phosphate according to any one of claims 1 to 4, characterized in that: The added amount of the cationic polyacrylamide is 10-30 mg / L.

7. The method for recovering iron phosphate according to any one of claims 1 to 4, characterized in that: The pH of the ferric phosphate filtrate was adjusted to 1.5-1.

8.

8. The method for recovering iron phosphate according to claim 2, characterized in that: The mass ratio of the precipitate to the mixed solution of ferrous sulfate and hydrochloric acid is 1:3-5; wherein the mass ratio of the ferrous sulfate to the hydrochloric acid is.

9. The method for recovering iron phosphate according to claim 8, characterized in that: The pH value of the mixed solution of ferrous sulfate and hydrochloric acid is 1.8-2.

0.

10. The method for recovering iron phosphate according to claim 8, characterized in that: The concentration of ferrous ions in the mixed solution of ferrous sulfate and hydrochloric acid is 20-100 mg / L.

Citation Information

Patent Citations

  • Efficient recycling method of waste residues after lithium extraction

    CN116854062A

  • Method for recovering resource

    JP2008195558A