SAPO-11 molecular sieve as well as preparation method and application thereof
The preparation of SAPO-11 molecular sieve through hydrothermal reaction using phosphorus source, aluminum source and structural guide agent, solved the problems of large size and high cost in the prior art, and achieved the preparation of SAPO-11 molecular sieve with small grain size and low cost. Suitable for industrial production and improves the service life of the catalyst.
Patent Information
- Application Number
- CN202310499248.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-05
AI Technical Summary
In the prior art, the preparation of SAPO-11 molecular sieve has problems of large size and high cost. Commonly used template agents and additives are not conducive to large-scale industrial production, and microwave method can easily lead to crystallization, affecting the preparation of pure phase molecular sieve.
Use phosphorus source, aluminum source, silicon source, structural guide agent N,N,N',N'-tetramethylhexanediamine or N,N,N',N'-tetramethylpentanediamine and imidazole compounds As a template agent, SAPO-11 molecular sieve is prepared through hydrothermal reaction, avoiding the use of surfactants and environmentally harmful substances, and achieving the goal of small grain size and low cost.
The prepared SAPO-11 molecular sieve has a small grain size and a long service life. The synthesis process is simple, economical and environmentally friendly, suitable for industrial applications, and significantly improves the service life of the catalyst.
Smart Images

Figure CN118894536A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of molecular sieve synthesis, and in particular to a SAPO-11 molecular sieve and a preparation method and application thereof. Background Art
[0002] Molecular sieves are a class of substances with uniform micropores, whose pore size is comparable to that of general molecules. They are widely used in the fields of petrochemicals, agriculture and animal husbandry, environmental protection, and high-tech and cutting-edge technologies. Since molecular sieves have uniform and regular pores, and the pore size is of the same order of magnitude as that of small organic molecules, in chemical reactions, the molecules entering the molecular sieve can be "screened" according to the spatial size of the molecules, thereby obtaining a certain selective adsorption and catalytic shape-selective effect. The framework of the molecular sieve is usually composed of coordinated tetrahedrons (TO4) connected by common vertices (usually oxygen atoms). For conventional zeolite molecular sieves, the tetrahedrons in the framework are mainly silicon-oxygen tetrahedrons and aluminum-oxygen tetrahedrons. These two tetrahedrons can also be replaced by other tetrahedrons, thereby forming many molecular sieves with various framework structures or various framework compositions.
[0003] In 1971, Flanigen et al. reported the synthesis of aluminum phosphate molecular sieves (Molecular Sieve Zeolites-I, ACS, Washingtom DC), which can be understood as the silicon oxygen tetrahedron in the zeolite molecular sieve is replaced by phosphorus oxygen tetrahedron to form a molecular sieve. The framework of this type of molecular sieve is composed of AlO4 - and PO4 +The whole molecular sieve framework is electrically neutral. Similar to zeolite molecular sieves, the aluminum oxygen tetrahedron or phosphorus oxygen tetrahedron in aluminum phosphate molecular sieves can also be replaced by other tetrahedrons, among which the most common are silicon oxygen tetrahedron and zinc oxygen tetrahedron. The introduction of these tetrahedrons gives aluminum phosphate molecular sieves new properties. Compared with zeolite molecular sieves, the artificial synthesis of aluminum phosphate molecular sieves was studied relatively late. Under hydrothermal synthesis conditions, the oxides of aluminum, silicon and phosphorus were mixed to obtain silicon phosphorus aluminum molecular sieves with the same crystal structure as analcime, chabazite, Phillipsite-harmotome, L-type molecular sieve, A-type molecular sieve and B-type molecular sieve, in which the phosphorus content is 5% to 25% (in terms of P2O5), but no molecular sieves different from the known zeolite molecular sieve structure were found. US 4310440 uses organic amine or quaternary ammonium compound as template, and hydrothermally synthesizes a series of aluminum phosphate molecular sieves, which include: AlPO4-5, AlPO4-8, AlPO4-9, AlPO4-11, AlPO4-12, AlPO4-14, AlPO4-16, AlPO4-17, AlPO4-18, AlPO4-20, AlPO4-21, AlPO4-22, AlPO4-23, AlPO4-25, AlPO4-26, AlPO4-28, AlPO4-31, etc. With the continuous deepening of the understanding of factors such as molecular sieve structure, performance, synthesis method, conditions, and the continuous progress of synthesis technology, molecular sieves of new structure are constantly being synthesized. With the development of industrial application, small crystals and crystal face control growth, for the synthesis of aluminum phosphate molecular sieve, the type of organic template is one of the key factors determining its structure. So far, organic amine is still the most widely used template in the synthesis of aluminum phosphate molecular sieve. Compared with silica-alumina zeolite molecular sieves, the industrial application of phosphate-alumina molecular sieves is still rare. Currently, only a few molecular sieves have been actually applied in industry, such as SAPO-34 and SAPO-11 molecular sieves.
[0004] In addition, in practical applications, it is precisely because of this "screening" function of molecular sieves that the mass transfer and heat transfer performance of the reaction are often limited, which in turn affects the activity and life of the catalyst. This deficiency can be further overcome by reducing the crystal size and adjusting the crystal pore structure. Therefore, the synthesis of small nano-crystals, nano-crystalline flakes and the introduction of mesopores to synthesize multi-level porous grains have aroused great interest among scientific researchers.
[0005] CN108996518A used solid acid to post-treat SAPO-11 molecular sieve under different conditions to obtain SAPO-11 molecular sieve with multi-level pore properties; CN109896531A used diethylamine and diisopropylamine as mixed templates and pre-treated the crystallization liquid with the help of a microwave reactor to prepare nanorod-shaped SAPO-11 molecular sieve. Master's thesis "Preparation of Ultrafine SAPO-11 Molecular Sieves and Study on Their Isomerization Performance" (China University of Petroleum, Han Lei, 2013.5) used hexadecyltrimethylammonium bromide (CTAB) and hydrofluoric acid (HF) as additives, and finally obtained ultrafine SAPO-11 molecular sieves with a size of 200nm by optimizing the synthesis conditions.
[0006] In the existing technology and research, the commonly used templates are diethylamine, dipropylamine or diisopropylamine. In order to reduce the grain size, expensive surfactants (such as hexadecyltrimethylammonium bromide), HF (aq) and other special additives are usually added, which is not conducive to industrial scale-up. Although the microwave method has great advantages in time cost, it is easy to cause crystallization during the crystallization process, generating AlPO-5 or CFSAPO-1 (C) impurities, which is not conducive to the preparation of pure phase SAPO-11 molecular sieves. At the same time, the microwave method is not conducive to industrial large-scale production.
[0007] In view of the shortcomings of the prior art, the present invention aims to propose a preparation method that is not involved in the prior art, does not require the addition of additional surfactants, and does not require the use of environmentally harmful substances. The raw materials are cheap and readily available, the operation is simple, the repeatability is good, and it is easy to industrialize and mass produce. Summary of the invention
[0008] The purpose of the present invention is to overcome the problems of large size and high preparation cost of SAPO-11 molecular sieve in the prior art, and to provide a SAPO-11 molecular sieve and a preparation method and application thereof. The SAPO-11 molecular sieve has the characteristics of small size and low preparation cost.
[0009] To achieve the above object, the first aspect of the present invention provides a SAPO-11 molecular sieve, which is a spherical aggregate with a diameter of 2-50 μm formed by primary nano-sheet crystals with a thickness of 15-60 nm, and a median pore size of 1550-1700 nm.
[0010] The second aspect of the present invention provides a method for preparing the molecular sieve of the present invention, which comprises preparing a hydrothermal reaction mixture with a phosphorus source, an aluminum source, a silicon source, a structure directing agent R1 and an additive R2, aging and crystallizing the reaction mixture, wherein the molar ratio of each substance is: (0.01-0.5) SiO2: (0.8-1.2) Al2O3: 1P2O5: (0.1-0.5) R1: (0.3-1.0) R2: (40-90) H2O; the structure directing agent R1 is selected from N,N,N',N'-tetramethylhexanediamine and / or N,N,N',N'-tetramethylpentanediamine; and the additive R2 is an imidazole compound.
[0011] The third aspect of the present invention provides an application of the molecular sieve of the present invention in catalyst preparation.
[0012] Through the above technical solution, the present invention has the following beneficial effects:
[0013] The invention provides a SAPO-11 molecular sieve with a small crystal size and a long service life.
[0014] The catalyst of the present invention is prepared by the method of the present invention. The synthesis process does not require ultrasonic or microwave treatment, and does not require the addition of complex organic surfactants and environmentally harmful substances such as HF, so that the preparation process is simple, economical, and environmentally friendly. The raw materials are cheap and easy to obtain, which has great advantages in actual industrial applications.
[0015] The molecular sieve of the present invention is used for catalyst preparation, which can significantly increase the service life of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is the XRD pattern of the molecular sieve of Example 1;
[0017] Figure 2 This is a SEM image of the molecular sieve of Example 1 magnified 40,000 times;
[0018] Figure 3 This is a SEM image of the molecular sieve of Example 1 magnified 2,000 times;
[0019] Figure 4 is the XRD pattern of the molecular sieve of Example 6;
[0020] Figure 5 This is a SEM image of the molecular sieve of Example 6 magnified 20,000 times;
[0021] Figure 6 This is a SEM image of the molecular sieve of Example 6 magnified 10,000 times;
[0022] Figure 7 is the XRD pattern of the molecular sieve of Comparative Example 1;
[0023] Figure 8 This is the SEM image of the molecular sieve of Comparative Example 1;
[0024] Fig. 9 This is the XRD pattern of the molecular sieve of Comparative Example 2. DETAILED DESCRIPTION
[0025] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0026] The first aspect of the present invention provides a SAPO-11 molecular sieve, which is a spherical aggregate with a diameter of 2-50 μm formed by primary nano-sheet crystals with a thickness of 15-60 nm. The median pore size of the molecular sieve is 1550-1700 nm.
[0027] The invention provides a SAPO-11 molecular sieve with a small crystal size and a long service life.
[0028] According to a preferred embodiment of the present invention, the molecular sieve is a spherical aggregate with a diameter of 20-40 μm formed by aggregation of primary nano-sheet crystals with a thickness of 20-45 nm, and the median pore size of the molecular sieve is 1600-1650 nm.
[0029] The molecular sieves having the aforementioned characteristics of the present invention can achieve the purpose of the present invention, and there is no special requirement for their preparation methods. According to the present invention, a preparation method of the molecular sieve of the present invention is provided, which comprises preparing a hydrothermal reaction mixture with a phosphorus source, an aluminum source, a silicon source, a structure directing agent R1 and an additive R2, aging and crystallizing the reaction mixture, wherein the molar ratio of each substance is: (0.01-0.5) SiO2: (0.8-1.2) Al2O3: 1P2O5: (0.1-0.5) R1: (0.3-1.0) R2: (40-90) H2O; the structure directing agent R1 is selected from N,N,N',N'-tetramethylhexanediamine and / or N,N,N',N'-tetramethylpentanediamine; and the additive R2 is an imidazole compound.
[0030] According to a preferred embodiment of the present invention, the molar ratio of each substance in the reaction mixture is: (0.05-0.3) SiO2: (0.8-1.0) Al2O3: 1P2O5: (0.2-0.5) R1: (0.3-1.0) R2: (50-75) H2O.
[0031] In the present invention, the silicon source may be a common silicon-containing compound in the art. According to a preferred embodiment of the present invention, the silicon source is selected from silica sol, fumed silica or a mixture thereof.
[0032] In the present invention, the aluminum source can be a common aluminum-containing compound in the art. According to a preferred embodiment of the present invention, the aluminum source is selected from at least one of pseudo-boehmite, aluminum isopropoxide, aluminum sulfate, aluminum chloride and aluminum hydroxide.
[0033] In the present invention, the phosphorus source may be a common phosphorus-containing compound in the art. According to a preferred embodiment of the present invention, the phosphorus source is selected from at least one of phosphoric acid, phosphorous acid, ammonium hydrogen phosphate and diammonium phosphate.
[0034] According to a preferred embodiment of the present invention, the imidazole compound is selected from at least one of imidazole, 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-butylimidazole, 1-(2-aminoethyl)imidazole and 1-(3-aminopropyl)imidazole.
[0035] In the present invention, the preparation step of the hydrothermal reaction mixture can be a conventional choice in the art. According to a preferred embodiment of the present invention, the preparation step of the hydrothermal reaction mixture is:
[0036] 1) dissolving an aluminum source and a phosphorus source in water to obtain a mixed solution I;
[0037] 2) adding a mixture of the template R1, the additive R2 and water to the mixed solution I to obtain a mixed solution II;
[0038] 3) Adding a silicon source to the mixed solution II to obtain a hydrothermal reaction mixed solution.
[0039] In the present invention, the aging conditions may be conventionally selected in the art. According to a preferred embodiment of the present invention, the aging conditions include: an aging temperature of 20-40° C. and an aging time of 2-15 h.
[0040] In the present invention, the crystallization conditions can be conventionally selected in the art. According to a preferred embodiment of the present invention, the crystallization conditions include: a crystallization temperature of 180-210°C, preferably 190-205°C; and / or a crystallization time of 2-36h, preferably 4-24h.
[0041] According to a preferred embodiment of the present invention, the aging and crystallization can be carried out in a crystallization kettle lined with polytetrafluoroethylene, preferably in a dynamic aging and crystallization manner, more preferably in an agitated condition.
[0042] According to a preferred embodiment of the present invention, the method further comprises cooling, separating, washing, drying and calcining the crystallized product.
[0043] In the present invention, the cooling, separation and washing can be conventionally selected in the art as long as the purpose of the present invention can be achieved.
[0044] In the present invention, the drying conditions can be conventionally selected in the art. According to a preferred embodiment of the present invention, the drying conditions include: a drying temperature of 50-200°C, preferably 80-120°C, and / or a drying time of 5-30h, preferably 8-15h.
[0045] In the present invention, the calcination conditions can be conventionally selected in the art. According to a preferred embodiment of the present invention, the calcination conditions include: a calcination temperature of 350-700°C, preferably 450-600°C; and / or a calcination time of 1-15h, preferably 5-8h.
[0046] The third aspect of the present invention provides an application of the molecular sieve of the present invention in catalyst preparation.
[0047] The molecular sieve of the present invention is used for catalyst preparation, which can significantly increase the service life of the catalyst.
[0048] The present invention will be described in detail below by way of examples. In the following examples, the structure of the molecular sieve is determined by an X-ray diffraction spectrum (XRD), and the X-ray diffraction spectrum (XRD) of the molecular sieve is determined by an X-ray powder diffraction (XRD) instrument, using a Cu-Kα ray source, with a Kα1 wavelength λ=1.5405980 angstroms. Nickel filter, working voltage 40kV, current 40mA, scanning range 3-50°. The product morphology was photographed by Japanese emission scanning electron microscope (Fe-SEM). The median pore size was determined by mercury intrusion type pore size analyzer, and its technical indicators are Pascal 140 low-pressure mercury intrusion instrument: pore size: 116~3.8μm, pressure range 0.1~400KPa; Pascal 240 high-pressure mercury intrusion instrument: pore size: 15~0.0074μm, maximum pressure 200MPa.
[0049] Phosphoric acid (85%), phosphorous acid, ammonium hydrogen phosphate (Shanghai test) and other raw materials, N,N,N',N'-tetramethylhexanediamine and / or N,N,N',N'-tetramethylpentanediamine (Wokai), aluminum isopropoxide (Shanghai test), nano-silica (Wokai) and the like are commercially available products of Sinopharm Chemical Reagent Co., Ltd.; imidazole chemically pure raw materials are commercially available products of Aladdin Reagent Co., Ltd.; pseudo-boehmite (alumina content of 70% on a dry basis) is commercially available product of Jiangsu Sanji Industrial Co., Ltd.; silicon source: HS Ludox-40% is from Sigma-Aldrich.
[0050] Example 1
[0051] Weigh 2.56g of pseudo-boehmite (70% on a dry basis, the same below), add 13g of water, then add 4.6g of 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.76g of 1-(3-aminopropyl)imidazole and 5g of water, and a mixture of 0.68g of N,N,N',N'-tetramethylhexanediamine and 5g of water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g of nano-silicon dioxide to mixed solution II, stir at 30°C overnight. Crystallize at 200°C for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110°C overnight and calcined at 550°C for 5h to obtain a molecular sieve. Figure 1 is the XRD pattern of the obtained molecular sieve, which can be seen to be SAPO-11 molecular sieve; Figure 2 (Magnified 40,000 times), Figure 3 (2000 times magnification) is the SEM image of the molecular sieve obtained by scanning electron microscope at different magnifications. It can be seen that the molecular sieve is a spherical aggregate of nanosheets. From the high-magnification scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The mercury intrusion pore size analyzer measured that the median pore size of the molecular sieve is 1639.93nm.
[0052] Example 2
[0053] Weigh 2.56g pseudo-boehmite, add 13g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.24g imidazole and 5g water, a mixture of 1.37g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g nano-silicon dioxide to mixed solution II, stir overnight at 30℃. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 6h to obtain a spherical SAPO-11 molecular sieve aggregated with nano-sheets. From the high-power scanning electron microscope, it can be seen that the thickness of the nano-sheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1637.89 nm.
[0054] Example 3
[0055] Weigh 2.91g pseudo-boehmite, add 23g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.76g 1-(3-aminopropyl) imidazole and 10g water, 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.48g nano-silicon dioxide to mixed solution II, stir overnight at 30℃. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 520℃ for 10h to obtain a spherical SAPO-11 molecular sieve with nano-sheets aggregated. From the high-power scanning electron microscope, it can be seen that the thickness of the nano-sheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1643.73 nm.
[0056] Example 4
[0057] Weigh 2.56g pseudo-boehmite, add 13g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.76g 1-(3-aminopropyl) imidazole and 5g water, 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.3g 40% silica sol (Ludox-40%) to mixed solution II, stir overnight at 30℃. Crystallize at 185℃ for 16h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain spherical SAPO-11 molecular sieves aggregated in nanosheets. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1641.37 nm.
[0058] Example 5
[0059] Weigh 3.2g of pseudo-boehmite, add 22g of water, then add 4.6g of 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.76g of 1-(3-aminopropyl)imidazole and 5g of water, 1.3g of N,N,N',N'-tetramethylpentanediamine and 5g of water to mixed solution I, stir at room temperature for 4h to obtain mixed solution II; then add 0.3g of 40% silica sol (Ludox-40%) to mixed solution II, stir overnight at 30℃. Crystallize at 205℃ for 4h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 600℃ for 2h to obtain a spherical SAPO-11 molecular sieve aggregated in nanosheets. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1642.61 nm.
[0060] Example 6
[0061] Weigh 2.56g of pseudo-boehmite, add 6g of water, then add 4.6g of 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 0.76g of 1-(3-aminopropyl)imidazole and 5g of water, 0.78g of N,N,N',N'-tetramethylpentanediamine and 5g of water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g of nano-silicon dioxide to mixed solution II, stir at 30℃ overnight. Crystallize at 190℃ for 12h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. Figure 4is the XRD pattern of the obtained molecular sieve, which can be seen to be SAPO-11 molecular sieve; Figure 5 (Magnified 20,000 times), Figure 6 (Magnified 10,000 times) are SEM images of the molecular sieve obtained by scanning electron microscope at different magnifications. It can be seen that the molecular sieve is a spherical aggregate of nanosheets. From the high-magnification scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The mercury intrusion pore size analyzer measured that the median pore size of the molecular sieve is 1639.67nm.
[0062] Example 7
[0063] Weigh 7.2g aluminum isopropoxide (purity 100%), add 13g water, stir at room temperature for 2h, fully hydrolyze, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h, and obtain mixed solution I; then add a mixture of 1.76g 1-(3-aminopropyl) imidazole and 5g water, 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h, and obtain mixed solution II; then add 0.36g nano-silicon dioxide to mixed solution II, stir at 30℃ overnight. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a spherical SAPO-11 molecular sieve with nano-sheet aggregation. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The mercury intrusion pore size analyzer measured that the median pore size of the molecular sieve is 1640.94nm.
[0064] Example 8
[0065] Weigh 2.56g pseudo-boehmite, add 13g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.24g imidazole and 5g water, 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g nano-silicon dioxide to mixed solution II, stir overnight at 30℃. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a spherical SAPO-11 molecular sieve aggregated with nano-sheets. From the high-power scanning electron microscope, it can be seen that the thickness of the nano-sheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1644.13 nm.
[0066] Example 9
[0067] Weigh 2.56g pseudo-boehmite, add 13g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 2g 1-propyl imidazole and 5g water, 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g nano-silicon dioxide to mixed solution II, stir overnight at 30℃. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a spherical SAPO-11 molecular sieve with nano-sheets aggregated. From the high-power scanning electron microscope, it can be seen that the thickness of the nano-sheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1644.73 nm.
[0068] Example 10
[0069] Weigh 2.56g pseudo-boehmite, add 13g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.49g 1-methylimidazole and 5g water, 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g nano-silicon dioxide to mixed solution II, stir overnight at 30℃. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a spherical SAPO-11 molecular sieve aggregated with nano-sheets. From the high-power scanning electron microscope, it can be seen that the thickness of the nano-sheets is in the range of 20-45nm, and the diameter of the spherical aggregates is in the range of 5-20μm. The median pore size of the molecular sieve measured by mercury intrusion pore size analyzer was 1645.03 nm.
[0070] Comparative Example 1
[0071] Weigh 2.56g pseudo-boehmite, add 13g water, then add 4.6g 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 0.68g N,N,N',N'-tetramethylhexanediamine and 5g water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g aerosol to mixed solution II, stir overnight. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. Figure 7 is the XRD pattern of the obtained molecular sieve, which can be seen to be SAPO-11 molecular sieve; Figure 8This is a SEM image of the molecular sieve obtained by scanning electron microscopy. It can be seen that the molecular sieve is a non-spherical aggregate composed of non-flaky grains slightly containing impurities.
[0072] Comparative Example 2
[0073] Weigh 2.56g of pseudo-boehmite, add 12.8g of water, then add 4.6g of 85% phosphoric acid, stir at room temperature for 2h to obtain mixed solution I; then add a mixture of 1.76g of aminopropyl imidazole and 10g of water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.12g of aerosol to mixed solution II, stir overnight. Crystallize at 200℃ for 6h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight to obtain a molecular sieve, Fig. 9 : is the XRD pattern of the obtained molecular sieve, it can be seen that the molecular sieve is not SAPO-11 molecular sieve.
[0074] It can be seen from the results of the examples that the molecular sieve of the present invention is a spherical aggregate with a diameter of 2-50 μm, which is composed of primary nano-sheet crystals with a thickness of 15-50 nm. The molecular sieve is small in size.
[0075] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A SAPO-11 molecular sieve, characterized in that: The molecular sieve is a spherical aggregate with a diameter of 2-50 μm formed by aggregation of primary nano-thin sheet crystals with a thickness of 15-60 nm. The median pore diameter of the molecular sieve is 1550-1700 nm.
2. The molecular sieve according to claim 1, wherein The molecular sieve is a spherical aggregate with a diameter of 20-40 μm formed by aggregation of primary nano-sheet crystal particles with a thickness of 20-45 nm, and the median pore diameter of the molecular sieve is 1600-1650 nm.
3. The method for preparing the molecular sieve according to claim 1 or 2, characterized in that: The method comprises preparing a hydrothermal reaction mixture with a phosphorus source, an aluminum source, a silicon source, a structure directing agent R1 and an additive R2, aging and crystallizing the reaction mixture, wherein the molar ratio of each substance is: (0.01-0.5) SiO2: (0.8-1.2) Al2O3: 1P2O5: (0.1-0.5) R1: (0.3-1.0) R2: (40-90) H2O; the structure directing agent R1 is selected from N,N,N',N'-tetramethylhexanediamine and / or N,N,N',N'-tetramethylpentanediamine; and the additive R2 is an imidazole compound.
4. The preparation method according to claim 3, wherein The molar ratio of each substance in the reaction mixture is: (0.05-0.3) SiO2: (0.8-1.0) Al2O3: 1P2O5: (0.2-0.5) R1: (0.3-1.0) R2: (50-75) H2O.
5. The preparation method according to claim 3 or 4, wherein The imidazole compound is selected from at least one of imidazole, 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-butylimidazole, 1-(2-aminoethyl)imidazole and 1-(3-aminopropyl)imidazole.
6. The preparation method according to any one of claims 3 to 5, wherein: The preparation steps of the hydrothermal reaction mixture are: 1) dissolving an aluminum source and a phosphorus source in water to obtain a mixed solution I; 2) adding a mixture of the template R1, the additive R2 and water to the mixed solution I to obtain a mixed solution II; 3) Adding a silicon source to the mixed solution II to obtain a hydrothermal reaction mixed solution.
7. The preparation method according to any one of claims 3 to 6, wherein: The aging conditions include: aging temperature of 20-40° C., aging time of 2-15 h; and / or The crystallization conditions include: a crystallization temperature of 180-210° C., preferably 190-205° C.; and / or a crystallization time of 2-36 h, preferably 4-24 h.
8. The preparation method according to any one of claims 3 to 7, wherein: The method further comprises cooling, separating, washing, drying and calcining the crystallized product.
9. The preparation method according to claim 8, wherein: The drying conditions include: a drying temperature of 50-200°C, preferably 80-120°C, and / or a drying time of 5-30h, preferably 8-15h; and / or The calcination conditions include: a calcination temperature of 350-700° C., preferably 450-600° C.; and / or a calcination time of 1-15 hours, preferably 5-8 hours.
10. Use of the molecular sieve according to claim 1 or 2 in the preparation of catalysts.
Citation Information
Patent Citations
Multi-stage porous SAPO-11 molecular sieve and synthesis method and application thereof
CN108996518A
Preparation method of SAPO-11 molecular sieve
CN109896531A
Crystalline metallophosphate compositions
US4310440A
Method for preparing nanosheet-shaped SAPO-11 molecular sieve through hydrothermal synthesis method
CN106517229A
Preparation method and application of microporous SAPO-11 molecular sieve
CN115072738A