Method for reducing residual alkali on surface of high-nickel ternary positive electrode material, prepared high-nickel ternary positive electrode material and lithium ion battery
By using alkaline washing liquid with a Li+ concentration of 500ppm to 3000ppm, the surface residual alkali problem is solved, the high-temperature circulation and storage performance of the material is improved, and the specific capacity and first charge and discharge efficiency of the material are ensured.
Patent Information
- Application Number
- CN202411327963.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The residual alkali on the surface of high-nickel ternary positive electrode material leads to a decline in material performance, especially high-temperature circulation and poor storage performance. The prior art such as water washing methods damage the specific capacity of the material and the first charge and discharge efficiency when removing alkaline substances.
采用Li+浓度为500ppm~3000ppm的碱性洗涤液与高镍三元正极材料混合搅拌,进行压滤和干燥后烧结,形成低残余碱的高镍正极材料,通过这种方法有效降低材料表面残余碱,并提高高温循环和存储性能。
Effectively dissolve LiOH and Li2CO3 on the surface of the material, reduce the precipitation of Li+, significantly improve the high-temperature cycling and high-temperature storage performance of high-nickel ternary cathode materials, while maintaining the specific capacity of the material.
Smart Images

Figure CN118894560A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, in particular to a method for reducing residual alkali on the surface of a high-nickel ternary positive electrode material. Background Art
[0002] Lithium Nickel Cobalt Manganese Oxide Material LiNi x Mn y Co z In O2 (x+y+z=1), the value of x is higher than 0.6, which is generally called high-nickel ternary positive electrode material. Ni acts as an active ingredient in the ternary positive electrode material. The higher the Ni content, the more electrons can participate in the electrochemical reaction, and the higher the material discharge capacity. With the country's increasing requirements for the energy density of power batteries and the introduction of subsidies and energy density linkage policies, the application and development of high-nickel ternary positive electrode materials have been greatly promoted. In the ternary material system, as the nickel content increases, the average valence of nickel gradually increases from +2 to +3. However, Ni 3+ The ion is not very stable in the air and can be easily reduced to Ni 2+ , accompanied by the precipitation of lithium, alkaline substances such as LiOH and Li2CO3 are generated on the surface of the particles. Too much residual lithium on the surface of the particles will bring many hazards. For example, too much residual lithium on the surface of the material will cause a higher pH value. Too much residual alkali will cause gelation of the slurry during the preparation of the electrode sheet, resulting in uneven slurry coating to form jelly, affecting the coating; resulting in poor high-temperature storage performance of the battery and severe swelling; resulting in poor high-temperature cycle performance of the power battery and cycle diving and other problems.
[0003] The commonly used method to reduce the residual alkali on the surface of high-nickel materials is mainly water washing. There are several methods for water washing: 1) More than 80% of companies or research institutions add high-nickel positive electrode materials and deionized water or mixed solvents into a water washing kettle, stir and wash, and then discharge the water. This method can effectively reduce the residual alkali on the surface of high-nickel materials, but the disadvantages of this method are also very obvious. During the water washing process, the LiOH and Li 2 CO 3 on the surface are continuously dissolved in water, and the Li + in the lattice is continuously migrated out, which eventually leads to a high Li 2 CO 3 on the surface of the material, a decrease in Li + in the lattice, and ultimately a low specific capacity of the material and poor high-temperature cycle; 2) Through water phase coating and then secondary sintering, although this method can be uniformly coated on the surface of the material, thereby improving the cycle performance of the material, the first charge and discharge efficiency of the positive electrode material is greatly reduced, and it is not suitable for the coating of high-nickel materials. Therefore, it is urgent to find a modification method to reduce the residual alkali on the surface of high-nickel ternary positive electrode materials, and improve the high-temperature cycle performance and high-temperature storage performance under the premise of ensuring the specific capacity and other performance of high-nickel ternary positive electrode materials. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for reducing the residual alkali on the surface of high-nickel ternary positive electrode materials, which can effectively reduce the residual alkali on the surface of the material and further improve the high-temperature cycle performance and high-temperature storage performance of the high-nickel ternary positive electrode materials.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a method for reducing the residual alkali on the surface of a high-nickel ternary positive electrode material, wherein the high-nickel ternary positive electrode material and a washing liquid are mixed and stirred evenly to form a slurry; the slurry is then filtered and dried, and the dried product is sintered to obtain a high-nickel ternary positive electrode material with low residual alkali; The washing liquid is an alkaline washing liquid having a Li + concentration of 500 ppm to 3000 ppm.
[0006] Furthermore, the washing liquid is prepared by adding LiOH·H 2 O to pure water. The alkaline washing liquid A is an alkaline washing liquid with LiOH and Li 2 CO 3 as main solutes.
[0007] Furthermore, the slurry is filtered and the filtrate is collected, and then the filtrate is prepared as a washing liquid.
[0008] Furthermore, the mass ratio of the high-nickel ternary positive electrode material to the washing liquid is 1:0.8-2.
[0009] Furthermore, the high-nickel ternary positive electrode material is mixed with the washing liquid and stirred for 5 to 20 minutes.
[0010] Furthermore, the high-nickel positive electrode material is Li1+xNiaCobMncN(1-abc)O2+y, wherein (-0.1)≤x≤0.1, a≥0.8, 0≤b≤0.15, 0≤c≤0.15, (-0.1)≤y≤0.1, and N is one or more of Al, Ti, Mg, Zr, B, and Ca.
[0011] Furthermore, the slurry is filtered using a positive pressure filter.
[0012] Furthermore, a double cone dryer, a plowshare dryer, a vibration dryer or a vacuum dryer is used for drying, the drying temperature is 100-300°C, and the time is 1-5 hours; the dried product is sintered in an oxygen atmosphere furnace, the sintering temperature is 200-600°C, and the time is 2-10 hours.
[0013] The high-nickel ternary positive electrode material with low residual alkali is prepared by the above-mentioned method for reducing the residual alkali on the surface of the high-nickel ternary positive electrode material.
[0014] A lithium ion battery comprises a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is made of the above-mentioned high-nickel ternary positive electrode material with low residual alkali.
[0015] The beneficial effects of the present invention are as follows: the present invention creatively adopts an alkaline washing solution with a Li + concentration of 500ppm to 3000ppm to wash the residual alkali on the surface of the high-nickel ternary positive electrode material, which can effectively dissolve the residual alkali (LiOH and Li 2 CO 3 ) on the surface of the high-nickel positive electrode material, and at the same time can effectively reduce the precipitation of Li + in the material lattice caused by the reaction of the positive electrode material with water, inhibit the dissolution of Li +, and further improve the high-temperature cycle performance and high-temperature storage performance of the high-nickel ternary positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a comparison diagram of the first charge and discharge curves of Examples 1, 2, 3 of the present invention and Comparative Examples 1, 2, 3; Figure 2 It is a comparison diagram of high temperature cycle performance curves of Examples 1, 2, 3 of the present invention and Comparative Examples 1, 2, 3; Figure 3 It is a comparison diagram of high temperature cycle DCR curves of Examples 1, 2, 3 of the present invention and Comparative Examples 1, 2, 3. DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Example
[0018] The crushed material of the high nickel ternary positive electrode material with the chemical composition of LiNi 0.83 Co 0.11 Mn 0.06 O 2 after primary sintering is selected as the raw material, and the mass ratio of the high nickel ternary positive electrode material to the washing liquid is 1:1; Weigh 4.5 kg of deionized water and add it to the stirrer, then weigh 30.23 g of LiOH·H 2 O (LiOH content ≥ 56.9%) and dissolve it in 500 g of deionized water and add it to the stirrer to prepare an alkaline washing solution with a Li + concentration of about 1000 ppm; Then adjust the speed to 80rpm, add 5kg of high-nickel ternary positive electrode material, quickly add the stirrer, adjust the speed to 150rpm, and stir for 10min; quickly transfer the slurry after stirring to a positive pressure filter, use 0.3MPa compressed air to filter for 15min, collect the clarified filtrate during the filtration process, and then test the alkali content and lithium content of the filtrate; The filtered material was sieved with a 10-mesh screen and then transferred to a vacuum drying oven with a vacuum degree ≥ 0.08 MPa and dried at 150°C for 2 hours. The dried material was then secondary sintered in an atmosphere furnace at a temperature of 200°C for 6 hours to obtain a finished high-nickel ternary positive electrode material with low residual alkali. Example
[0019] The crushed material of the high-nickel ternary cathode material with a chemical composition of LiNi 0.83 Co 0.11 Mn 0.06 O 2 after primary sintering was selected as the raw material, and LiOH·H 2 O was added to deionized water to prepare an alkaline washing solution with a Li + concentration of about 2500ppm, and the mass ratio of the high-nickel ternary cathode material to the washing solution was 1:1.5; 7.5kg of the alkaline washing solution was weighed and added to the stirrer, and then the speed was adjusted to 80rpm, 5kg of the high-nickel ternary cathode material was added, and the stirrer was quickly added, and the speed was adjusted to 150rpm, and stirred for 10min; the slurry after stirring was quickly transferred to a positive pressure filter, and filtered with 0.3MPa compressed air for 15min, and the clarified filtrate was collected during the filtration process, and then the alkali content and lithium content of the filtrate were detected; The filtered material was sieved with a 10-mesh screen and then transferred to a vacuum drying oven with a vacuum degree ≥ 0.08 MPa and dried at 150°C for 2 hours. The dried material was then secondary sintered in an atmosphere furnace at a temperature of 200°C for 6 hours to obtain a finished high-nickel ternary positive electrode material with low residual alkali. Example
[0020] The crushed material of the high-nickel ternary positive electrode material with a chemical composition of LiNi 0.83 Co 0.11 Mn 0.06 O 2 after primary sintering is selected as the raw material, the filtrate obtained in Example 1 is added with ionized water to prepare an alkaline washing liquid with a Li + concentration of about 1000ppm, and the mass ratio of the high-nickel ternary positive electrode material to the washing liquid is 1:1; 5kg of the alkaline washing liquid is weighed and added to the stirrer, and then the speed is adjusted to 80rpm, 5kg of the high-nickel ternary positive electrode material is added, and the stirrer is quickly added, and the speed is adjusted to 150rpm, and stirred for 10min; the slurry after stirring is quickly transferred to a positive pressure filter, and compressed air of 0.3MPa is used for pressure filtration for 15min, and the clarified filtrate is collected during the pressure filtration process, and then the alkali content and lithium content of the filtrate are detected; The filtered material was sieved with a 10-mesh screen and then transferred to a vacuum drying oven with a vacuum degree ≥ 0.08 MPa and dried at 150°C for 2 hours. The dried material was then secondary sintered in an atmosphere furnace at a temperature of 200°C for 6 hours to obtain a finished high-nickel ternary positive electrode material with low residual alkali.
[0021] Comparative Example 1: The crushed material of the high-nickel ternary cathode material with a chemical composition of LiNi 0.83 Co 0.11 Mn 0.06 O 2 after primary sintering was selected as the raw material, and pure deionized water was used as the washing liquid, and the mass ratio of the high-nickel ternary cathode material to the washing liquid was 1:1; 5 kg of the washing liquid was weighed and added to the agitator, and then the speed was adjusted to 80 rpm, 5 kg of the high-nickel ternary cathode material was added, and the agitator was quickly added, and the speed was adjusted to 150 rpm, and stirred for 10 minutes; the slurry after stirring was quickly transferred to a positive pressure filter, and compressed air of 0.3 MPa was used for pressure filtration for 15 minutes, and the clarified filtrate was collected during the pressure filtration process, and then the alkali content and lithium content of the filtrate were detected; The filtered material was sieved with a 10-mesh screen and then transferred to a vacuum drying oven with a vacuum degree ≥ 0.08 MPa and dried at 150°C for 2 hours. The dried material was then secondary sintered in an atmosphere furnace at a temperature of 200°C for 6 hours to obtain a finished high-nickel ternary positive electrode material with low residual alkali.
[0022] Comparative Example 2: The crushed material of the high-nickel ternary positive electrode material with a chemical composition of LiNi 0.83 Co 0.11 Mn 0.06 O 2 after primary sintering is selected as the raw material, the filtrate obtained in Example 1 is added with ionized water to prepare an alkaline washing liquid with a Li + concentration of about 300 ppm, and the mass ratio of the high-nickel ternary positive electrode material to the washing liquid is 1:1; 5 kg of the alkaline washing liquid is weighed and added to the stirrer, and then the speed is adjusted to 80 rpm, 5 kg of the high-nickel ternary positive electrode material is added, and the stirrer is quickly added, and the speed is adjusted to 150 rpm, and stirred for 10 minutes; the slurry after stirring is quickly transferred to a positive pressure filter, and compressed air of 0.3 MPa is used for pressure filtration for 15 minutes, and the clarified filtrate is collected during the pressure filtration process, and then the alkali content and lithium content of the filtrate are detected; The filtered material was sieved with a 10-mesh screen and then transferred to a vacuum drying oven with a vacuum degree ≥ 0.08 MPa and dried at 150°C for 2 hours. The dried material was then secondary sintered in an atmosphere furnace at a temperature of 200°C for 6 hours to obtain a finished high-nickel ternary positive electrode material with low residual alkali.
[0023] Comparative Example 3: The crushed material of the high-nickel ternary positive electrode material with a chemical composition of LiNi 0.83 Co 0.11 Mn 0.06 O 2 after primary sintering is selected as the raw material, the filtrate obtained in Example 1 is added with ionized water to prepare an alkaline washing liquid with a Li + concentration of about 3500ppm, and the mass ratio of the high-nickel ternary positive electrode material to the washing liquid is 1:1; 5kg of the alkaline washing liquid is weighed and added to the stirrer, and then the speed is adjusted to 80rpm, 5kg of the high-nickel ternary positive electrode material is added, and the stirrer is quickly added, and the speed is adjusted to 150rpm, and stirred for 10min; the slurry after stirring is quickly transferred to a positive pressure filter, and compressed air of 0.3MPa is used for pressure filtration for 15min, and the clarified filtrate is collected during the pressure filtration process, and then the alkali content and lithium content of the filtrate are detected; The filtered material was sieved with a 10-mesh screen and then transferred to a vacuum drying oven with a vacuum degree ≥ 0.08 MPa and dried at 150°C for 2 hours. The dried material was then secondary sintered in an atmosphere furnace at a temperature of 200°C for 6 hours to obtain a finished high-nickel ternary positive electrode material with low residual alkali.
[0024] The filtrates obtained in Examples 1-3 and Comparative Examples 1-3 were tested for alkali content and lithium content, and the surface residual alkali and specific surface area of the dried products were tested. The results are shown in the following table: Alkali content test: The chemical reagent potentiometric titration method is used to test the content of LiOH and Li 2 CO 3. For the test of the alkali content of the powder material, first weigh 30g of the material and mix it with 100mL of pure water and stir it for 30min, filter to obtain a clear liquid, take 10mL of the liquid and titrate it with 0.05mol / L standard solution HCl, and calculate the amount of LiOH and Li 2 CO 3; for the test of the alkali content of the filtrate, directly take 10mL of the filtrate and titrate it with 0.05mol / L standard solution HCl, and calculate the amount of LiOH and Li2 CO 3.
[0025] Specific surface area test: In a liquid nitrogen environment, after measuring the amount of gas adsorbed on the solid surface at different relative pressures, the monolayer adsorption amount of the sample is obtained based on the Brownauer-Etter-Taylor (BET) multilayer adsorption theory and its formula, thereby calculating the specific surface area of the solid.
[0026] It can be seen from Table 1 that the lithium content in the low residual alkali high nickel ternary positive electrode material after drying of Examples 1-3 is greater than 7.01%, and the specific surface area is 0.89-0.91m2 / g, which significantly increases the specific surface area of the material without causing corrosion to the inside of the material. However, after the high nickel ternary positive electrode material in Comparative Example 1 is washed with water, the lithium hydroxide content on the surface of the material after drying is only 0.1190%, and the specific surface area is about 0.3m2 / g higher than that of the embodiment, indicating that the internal corrosion of the material is serious during the washing process, and the lithium inside the material is lost.
[0027] Button performance test: The high nickel ternary positive electrode materials with low residual alkali obtained in Examples 1-3 and Comparative Examples 1-3 were made into positive electrodes of 2025 button batteries, and then 2025 button batteries were made to conduct electrochemical performance tests. The test conditions were: Positive electrode: SP: PVDF = 90: 5: 5; Negative electrode: metallic lithium; Electrolyte: Xinzhoubang (M10); Charge and discharge voltage range 3.0-4.3V (nominal capacity 190mAh / g); High temperature cycle DCR performance test: The battery was first charged and discharged three times at 0.1C, and then the cycle performance was tested at 1C rate at room temperature (25℃) and high temperature (45℃). During the high-temperature cycle, the discharge voltage was recorded every minute, and the internal resistance change of the material during the high-temperature cycle was calculated using the voltage drop, and the DCR change curve was drawn. The results are shown in Figure 2. Figure 3 shown.
[0028] First charge and discharge test: The button cells made of high nickel ternary positive electrode materials of Examples 1-3 and Comparative Examples 1-3 were subjected to the first charge and discharge experiment. The test method was as follows: at a rate of 2.8-4.3V 0.1C (theoretical capacity is designed to be 200mAh / g), first 0.1C charging and then 0.1C discharging were performed to obtain the charge and discharge curve, and the first charge and discharge capacity was obtained.
[0029] High temperature cycle performance test: The button cells made of the high-nickel ternary positive electrode materials of Examples 1-3 and Comparative Examples 1-3 were subjected to a high-temperature (45°C) cycle performance experiment. The test method was as follows: after the first charge and discharge at 2.8-4.3V 0.1C (nominal capacity of 200mAh / g), the charge and discharge test was performed at a rate of 1C for 50 cycles to obtain the capacity retention rate after 50 high-temperature cycles. An alkaline washing solution with a Li+ concentration of 500ppm to 3000ppm was used to wash the residual alkali on the surface of the high-nickel ternary positive electrode material, which can effectively wash the residual alkali on the surface of the positive electrode material and prevent the migration of Li+ from the lattice clock, thereby ensuring the low specific capacity and high-temperature cycle performance of the high-nickel ternary positive electrode material. The capacity retention rate after 50 high-temperature cycles was greater than 88.6%, and the DCR growth rate after 50 high-temperature cycles was not greater than 212.8%.
Claims
1. A method for reducing residual alkali on the surface of high-nickel ternary positive electrode materials, Features: The high-nickel ternary positive electrode material and the washing liquid are mixed and stirred evenly to form a slurry; the slurry is then filtered and dried, and the dried product is sintered to obtain a high-nickel ternary positive electrode material with low residual alkali; The washing liquid is an alkaline washing liquid having a Li + concentration of 500 ppm to 3000 ppm.
2. A method for reducing residual alkali on the surface of a high-nickel ternary positive electrode material according to claim 1, Features: The washing liquid is pure water with LiOH·H 2 O prepared.
3. A method for reducing residual alkali on the surface of high-nickel ternary positive electrode materials according to claim 1, Features: The slurry is filtered and the filtrate is collected, and then the filtrate is prepared as a washing liquid.
4. A method for reducing residual alkali on the surface of a high-nickel ternary positive electrode material according to claim 1, Features: The mass ratio of the high-nickel ternary positive electrode material to the washing liquid is 1:0.8-2.
5. A method for reducing residual alkali on the surface of high-nickel ternary positive electrode materials according to claim 1, Features: Mix the high-nickel ternary positive electrode material with the washing liquid and stir for 5 to 20 minutes.
6. A method for reducing residual alkali on the surface of a high-nickel ternary positive electrode material according to claim 1, Features: The high-nickel positive electrode material is Li1+xNiaCobMncN(1-abc)O2+y, wherein (-0.1)≤x≤0.1, a≥0.8, 0≤b≤0.15, 0≤c≤0.15, (-0.1)≤y≤0.1, and N is one or more of Al, Ti, Mg, Zr, B, and Ca.
7. A method for reducing residual alkali on the surface of a high-nickel ternary positive electrode material according to claim 1, Features: The slurry is filtered using a positive pressure filter.
8. A method for reducing residual alkali on the surface of high-nickel ternary positive electrode materials according to claim 1, Features: The dried product is dried using a double cone dryer, a plowshare dryer, a vibration dryer or a vacuum dryer at a drying temperature of 100 to 300° C. and a time of 1 to 5 hours; the dried product is sintered in an oxygen atmosphere furnace at a sintering temperature of 200 to 600° C. and a time of 2 to 10 hours.
9. A high nickel ternary positive electrode material with low residual alkali obtained by the method for reducing residual alkali on the surface of a high nickel ternary positive electrode material according to claims 1 to 8.
10. A lithium ion battery comprising a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, and an electrolyte, Features: The positive electrode is made of the high-nickel ternary positive electrode material with low residual alkali as described in Claim 9.