High-temperature-resistant carbon fiber composite material and preparation process thereof

By using a combination of carbon fiber preforms, inert gases, slurries and adhesives in high-temperature resistant carbon fiber composites, combining high-temperature puncture and phosphoric acid solution soaking, the existing materials are solved at high temperatures by using high-efficiency initiators to eliminate small molecule residues. Creep problem significantly improves overall high temperature resistance and adhesive effect.

CN118894730APending Publication Date: 2024-11-05SHANGHAI CARBON BEAM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145166.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing high-temperature resistant carbon fiber composites are prone to creep in high-temperature environments, resulting in a reduced adhesion effect and insufficient overall high-temperature resistance.

Method used

Using a combination of carbon fiber preforms, inert gases, slurries and adhesives, the weight average molecular weight of the polymer is increased by puncture operation and soaking of phosphoric acid solution at high temperatures. , reduce the residue of small molecular weight substances and enhance the adhesion effect.

Benefits of technology

It effectively improves the overall high-temperature resistance of the composite material, enhances the adhesion effect, and ensures stability and performance under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002009490000081
    Figure BDA0005002009490000081
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant carbon fiber composite material and a preparation process thereof, and relates to the technical field of carbon fiber composite materials. The high-temperature-resistant carbon fiber composite material is prepared from the following components in parts by mass: 70-80 parts of a carbon fiber preform; 1-2 parts of inert gas; 10 to 15 parts of slurry; 8-9 parts of an adhesive; according to the invention, the composite material is bonded by using the slurry, so that the overall high-temperature resistance of the composite material can be effectively improved, and meanwhile, in the preparation process, the benzoyl peroxide initiator with higher decomposition temperature is adopted for initiation in the early stage, and the azodiisobutyronitrile initiator is adopted for reflux polymerization in the later stage of the reaction, so that the residual monomers can be effectively eliminated; the weight-average molecular weight of the polymer is improved, and residues generated by creep of small molecular weight substances in the adhesive under a high-temperature condition are reduced, so that the bonding effect of the adhesive is further ensured, and the high-temperature resistance of the composite material is further ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of carbon fiber composite materials, and in particular, relates to a high temperature resistant carbon fiber composite material and a preparation process thereof. Background Art

[0002] Carbon fiber has many excellent properties, including high axial strength and modulus, low density, high specific performance, no creep, ultra-high temperature resistance in non-oxidizing environment, good fatigue resistance, specific heat and electrical conductivity between non-metal and metal, small thermal expansion coefficient and anisotropy, good corrosion resistance, good X-ray transmittance, good electrical and thermal conductivity, good electromagnetic shielding, etc. The finished carbon fiber board prepared from carbon fiber, currently known carbon fiber board has the characteristics of high specific strength, large specific modulus, good corrosion resistance and durability, small expansion coefficient and low production cost.

[0003] The existing patent CN113105717B discloses a high-temperature resistant carbon fiber composite material and a preparation method thereof, comprising epoxy resin glue, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, chitosan composite, and carbon fiber; chitosan is used to bond the carbon fiber and the resin matrix, and tetraaminophthalocyanine copper prepared by 4-nitrophthalimide is added, the amino group on the tetraaminophthalocyanine copper can form a covalent bond between the carbon fiber and the epoxy resin and participate in the curing of the epoxy resin, thereby strengthening the interface crosslinking density between the carbon fiber and the epoxy resin, and at the same time, since the tetraaminophthalocyanine copper has a rigid aromatic heterocyclic structure, the strength of the interface is improved, the glass transition temperature of the interface is increased, and the high temperature resistance of the composite material is improved; the composite material prepared by the present invention has good practicality and production value by strengthening the interface crosslinking and strength between the carbon fiber and the resin matrix, increasing the glass transition temperature of the interface, and improving the high temperature resistance of the composite material.

[0004] However, the carbon fiber composite materials in the prior art still have certain shortcomings. In the above-mentioned scheme, the carbon fiber composite materials with small molecular weight are prone to creep under high temperature environment, which may lead to reduced bonding effect of multi-layer carbon fiber plain fabrics. The overall high temperature resistance of carbon fiber composite materials needs to be further improved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a high temperature resistant carbon fiber composite material and a preparation process thereof which can overcome the above problems or at least partially solve the above problems.

[0006] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is: a high temperature resistant carbon fiber composite material, composed of the following mass components:

[0007] 70-80 parts of carbon fiber preform;

[0008] 1-2 parts of inert gas;

[0009] 10-15 parts of slurry;

[0010] 8-9 parts of adhesive.

[0011] Furthermore, the carbon fiber preform is a plain weave cloth woven from carbon fibers.

[0012] Preferably, the inert gas is argon.

[0013] Furthermore, the slurry is composed of the following components by mass: 60-65 parts of water, 35-40 parts of zirconium phosphate, and 5-8 parts of additives. The preparation steps of the slurry are as follows:

[0014] Step 1: Take water and put it into the mixing barrel;

[0015] Step 2: Put the weighed zirconium phosphate into a mixing bucket and stir thoroughly for 30-40 minutes;

[0016] Step 3: Add 5-8 parts of the weighed additive into the mixing tank, and heat and stir thoroughly for 8-10 minutes;

[0017] Step 4: Pour out the prepared slurry after cooling.

[0018] Furthermore, the mass ratio of zirconium phosphate to water in step 2 is 35:100.

[0019] Furthermore, the adhesive is composed of the following components by mass: 20-25 parts of butyl acrylate, 20-25 parts of ethyl acetate, 5-10 parts of aluminum oxide, 5-10 parts of silicon micropowder, 10-15 parts of initiator, and 8-10 parts of auxiliary agent;

[0020] The initiator includes benzoyl peroxide and azobisisobutyronitrile;

[0021] The specific preparation steps of the adhesive are as follows:

[0022] Step A1, weigh butyl acrylate and ethyl acetate and put them into a reaction tank;

[0023] Step A2, adding benzoyl peroxide into a reaction tank to initiate a reaction;

[0024] Step A3: After a period of reaction, azobisisobutyl cyanide is added to the reaction tank for secondary initiation to obtain a base liquid;

[0025] Step A4, adding butyl acrylate and ethyl acetate in an amount equal to that in step A1 into the reaction tank again for reaction;

[0026] Step A5, raising the temperature to 80-90° C., and adding azobisisobutyronitrile dropwise into the reaction tank again;

[0027] Step A6, after the heat preservation is completed, the remaining ethyl acetate is added to cool down to obtain a finished adhesive product.

[0028] A method for preparing a high temperature resistant carbon fiber composite material, comprising the following steps:

[0029] Step S1, placing the woven plain fabric in a vacuum furnace and heating it in an inert gas atmosphere;

[0030] Step S2, after keeping warm for 2 hours, cool to room temperature and take out;

[0031] Step S3, uniformly coating the prepared slurry and adhesive on the processed carbon fiber plain weave cloth;

[0032] Step S4, stacking and laying multiple groups of carbon fiber plain weave fabrics coated with slurry and adhesive;

[0033] Step S5, performing a puncture operation on the carbon fiber plain weave fabric in step S4;

[0034] Step S6, soaking the composite material in a phosphoric acid solution for 1-2 hours;

[0035] Step S7, taking out the soaked composite material and heating it to 600° C.;

[0036] Step S8, placing the composite material in step S7 into a high temperature furnace, heating to 900° C. in an inert gas protective atmosphere, keeping the temperature for 2 hours, and cooling to obtain a high temperature resistant composite material.

[0037] Furthermore, the coating thickness of the slurry and adhesive in step S3 is 1-10 microns.

[0038] Furthermore, in the step S5, when the composite material is punctured, the operating environment is 500-600°C.

[0039] Furthermore, the inert gas in step S8 is nitrogen.

[0040] After adopting the above technical scheme, the present invention uses slurry to bond the composite material, thereby effectively improving the overall high temperature resistance of the composite material. At the same time, in the preparation process, a benzoyl peroxide initiator with a higher decomposition temperature is used in the early stage to initiate the reaction, and azobisisobutyronitrile initiator is used for reflux polymerization in the later stage of the reaction, thereby effectively eliminating the remaining monomers, increasing the weight-average molecular weight of the polymer, and reducing the residues caused by creep of small molecular weight substances in the adhesive under high temperature conditions, thereby further ensuring the bonding effect of the adhesive, and further ensuring the high temperature resistance of the composite material. DETAILED DESCRIPTION

[0041] Embodiment 1:

[0042] A high temperature resistant carbon fiber composite material, consisting of the following quality components:

[0043] 75 carbon fiber preforms;

[0044] 2 parts of inert gas;

[0045] 12 parts of slurry;

[0046] 8 parts of adhesive.

[0047] The carbon fiber preform is a plain weave fabric woven from carbon fibers.

[0048] The inert gas is argon.

[0049] The slurry is composed of the following mass components: 62 parts of water, 35 parts of zirconium phosphate, and 6 parts of additives. The preparation steps of the slurry are as follows:

[0050] Step 1: Take water and put it into the mixing barrel;

[0051] Step 2: Put the weighed zirconium phosphate into a mixing bucket and stir thoroughly for 35 minutes;

[0052] Step 3: Add 6 parts of the weighed additive into the mixing tank, and heat and stir thoroughly for 9 minutes;

[0053] Step 4: Pour out the prepared slurry after cooling.

[0054] The mass ratio of zirconium phosphate to water in step 2 is 35:100.

[0055] The adhesive is composed of the following components by mass: 22 parts of butyl acrylate, 23 parts of ethyl acetate, 8 parts of aluminum oxide, 8 parts of silicon micropowder, 12 parts of initiator, and 9 parts of auxiliary agent;

[0056] The auxiliary agent is a thickener;

[0057] Initiators include benzoyl peroxide and azobisisobutyronitrile;

[0058] The specific preparation steps of the adhesive are as follows:

[0059] Step A1, weigh butyl acrylate and ethyl acetate and put them into a reaction tank;

[0060] Step A2, adding benzoyl peroxide into a reaction tank to initiate a reaction;

[0061] Step A3: After a period of reaction, azobisisobutyl cyanide is added to the reaction tank for secondary initiation to obtain a base liquid;

[0062] Step A4, adding butyl acrylate and ethyl acetate in an amount equal to that in step A1 into the reaction tank again for reaction;

[0063] Step A5, raising the temperature to 85° C., and adding azobisisobutyronitrile dropwise into the reaction tank again;

[0064] Step A6, after the heat preservation is completed, the remaining ethyl acetate is added to cool down to obtain a finished adhesive product.

[0065] A method for preparing a high temperature resistant carbon fiber composite material, comprising the following steps:

[0066] Step S1, placing the woven plain fabric in a vacuum furnace and heating it in an inert gas atmosphere;

[0067] Step S2, after keeping warm for 2 hours, cool to room temperature and take out;

[0068] Step S3, uniformly coating the prepared slurry and adhesive on the processed carbon fiber plain weave cloth;

[0069] Step S4, stacking and laying multiple groups of carbon fiber plain weave fabrics coated with slurry and adhesive;

[0070] Step S5, performing a puncture operation on the carbon fiber plain weave fabric in step S4;

[0071] Step S6, soaking the composite material in a phosphoric acid solution for 1.5 hours;

[0072] Step S7, taking out the soaked composite material and heating it to 600° C.;

[0073] Step S8, placing the composite material in step S7 into a high temperature furnace, heating to 900° C. in an inert gas protective atmosphere, keeping the temperature for 2 hours, and cooling to obtain a high temperature resistant composite material.

[0074] The coating thickness of the slurry and adhesive in step S3 is 1-10 microns.

[0075] When the composite material is punctured in step S5, the operating environment is 550°C.

[0076] The inert gas in step S8 is nitrogen.

[0077] Embodiment 2:

[0078] A high temperature resistant carbon fiber composite material, consisting of the following quality components:

[0079] 75 carbon fiber preforms;

[0080] 2 parts of inert gas;

[0081] 12 parts of slurry.

[0082] The carbon fiber preform is a plain weave fabric woven from carbon fibers.

[0083] The inert gas is argon.

[0084] The slurry is composed of the following mass components: 62 parts of water, 35 parts of zirconium phosphate, and 6 parts of additives. The preparation steps of the slurry are as follows:

[0085] Step 1: Take water and put it into the mixing barrel;

[0086] Step 2: Put the weighed zirconium phosphate into a mixing bucket and stir thoroughly for 35 minutes;

[0087] Step 3: Add 6 parts of the weighed additive into the mixing tank, and heat and stir thoroughly for 9 minutes;

[0088] Step 4: Pour out the prepared slurry after cooling.

[0089] The mass ratio of zirconium phosphate to water in step 2 is 35:100.

[0090] A method for preparing a high temperature resistant carbon fiber composite material, comprising the following steps:

[0091] Step S1, placing the woven plain fabric in a vacuum furnace and heating it in an inert gas atmosphere;

[0092] Step S2, after keeping warm for 2 hours, cool to room temperature and take out;

[0093] Step S3, uniformly coating the prepared slurry on the processed carbon fiber plain cloth;

[0094] Step S4, stacking and laying a plurality of groups of carbon fiber plain weave fabrics coated with slurry;

[0095] Step S5, performing a puncture operation on the carbon fiber plain weave fabric in step S4;

[0096] Step S6, soaking the composite material in a phosphoric acid solution for 1.5 hours;

[0097] Step S7, taking out the soaked composite material and heating it to 600° C.;

[0098] Step S8, placing the composite material in step S7 into a high temperature furnace, heating to 900° C. in an inert gas protective atmosphere, keeping the temperature for 2 hours, and cooling to obtain a high temperature resistant composite material.

[0099] The coating thickness of the slurry and adhesive in step S3 is 1-10 microns.

[0100] When the composite material is punctured in step S5, the operating environment is 550°C.

[0101] The inert gas in step S8 is nitrogen.

[0102] Embodiment 3:

[0103] A high temperature resistant carbon fiber composite material, consisting of the following quality components:

[0104] 75 carbon fiber preforms;

[0105] 2 parts of inert gas;

[0106] 8 parts of adhesive.

[0107] The carbon fiber preform is a plain weave fabric woven from carbon fibers.

[0108] The inert gas is argon.

[0109] The adhesive is composed of the following components by mass: 22 parts of butyl acrylate, 23 parts of ethyl acetate, 8 parts of aluminum oxide, 8 parts of silicon micropowder, 12 parts of initiator, and 9 parts of auxiliary agent;

[0110] The auxiliary agent is a thickener;

[0111] Initiators include benzoyl peroxide and azobisisobutyronitrile;

[0112] The specific preparation steps of the adhesive are as follows:

[0113] Step A1, weigh butyl acrylate and ethyl acetate and put them into a reaction tank;

[0114] Step A2, adding benzoyl peroxide into a reaction tank to initiate a reaction;

[0115] Step A3: After a period of reaction, azobisisobutyl cyanide is added to the reaction tank for secondary initiation to obtain a base liquid;

[0116] Step A4, adding butyl acrylate and ethyl acetate in an amount equal to that in step A1 into the reaction tank again for reaction;

[0117] Step A5, raising the temperature to 85° C., and adding azobisisobutyronitrile dropwise into the reaction tank again;

[0118] Step A6, after the heat preservation is completed, the remaining ethyl acetate is added to cool down to obtain a finished adhesive product.

[0119] A method for preparing a high temperature resistant carbon fiber composite material, comprising the following steps:

[0120] Step S1, placing the woven plain fabric in a vacuum furnace and heating it in an inert gas atmosphere;

[0121] Step S2, after keeping warm for 2 hours, cool to room temperature and take out;

[0122] Step S3, evenly coating the prepared adhesive on the processed carbon fiber plain weave cloth;

[0123] Step S4, stacking and laying a plurality of groups of carbon fiber plain weave fabrics coated with adhesive;

[0124] Step S5, performing a puncture operation on the carbon fiber plain weave fabric in step S4;

[0125] Step S6, soaking the composite material in a phosphoric acid solution for 1.5 hours;

[0126] Step S7, taking out the soaked composite material and heating it to 600° C.;

[0127] Step S8, placing the composite material in step S7 into a high temperature furnace, heating to 900° C. in an inert gas protective atmosphere, keeping the temperature for 2 hours, and cooling to obtain a high temperature resistant composite material.

[0128] The coating thickness of the slurry and adhesive in step S3 is 1-10 microns.

[0129] When the composite material is punctured in step S5, the operating environment is 550°C.

[0130] The inert gas in step S8 is nitrogen.

[0131] Comparative Example:

[0132] A high temperature resistant carbon fiber composite material, which is basically the same as Example 1, except that the mass components of the composite material are:

[0133] 80 carbon fiber preforms;

[0134] 1 part of inert gas;

[0135] 15 parts of slurry;

[0136] Adhesive 9 parts.

[0137] In combination with Examples 1 to 3 and the comparative example, the carbon fiber composite materials prepared in each group of Examples and the comparative example were tested, and the specific experimental steps are as follows:

[0138] Experiment 1:

[0139] Take Examples 1-3 and Comparative Example as experimental samples, make the samples into sizes of 15mm*15mm*3mm in length, width and height respectively, place them in an oven, raise the temperature to 150°C, measure the shear strength of the samples, and record;

[0140] Experiment 2:

[0141] Using Examples 1-3 and the comparative example as experimental samples, the samples were tested according to GB / T 2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method Part 2: Room Temperature Test" and the data were recorded;

[0142] Experiment 3:

[0143] Using Examples 1-3 and the comparative example as experimental samples, the samples were tested according to GB / T 15738-1995 "Test method for electrical conductivity of conductive and antistatic fiber reinforced plastics", and the data were recorded.

[0144] See Table 1 for specific test data:

[0145]

[0146] Table 1

[0147] In summary, referring to Table 1 and Examples 1-3, the present invention uses slurry to bond the composite material, thereby effectively improving the overall high temperature resistance of the composite material. At the same time, in the preparation process, a benzoyl peroxide initiator with a higher decomposition temperature is used in the early stage to initiate the reaction, and azobisisobutyronitrile initiator is used for reflux polymerization in the later stage of the reaction, thereby effectively eliminating the remaining monomers, increasing the weight-average molecular weight of the polymer, and reducing the residues caused by creep of small molecular weight substances in the adhesive under high temperature conditions, thereby further ensuring the bonding effect of the adhesive, and further ensuring the high temperature resistance of the composite material.

[0148] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.

Claims

1. A high temperature resistant carbon fiber composite material, characterized in that: It is composed of the following quality components: 70-80 parts of carbon fiber preform; 1-2 parts of inert gas; 10-15 parts of slurry; 8-9 parts of adhesive.

2. The high temperature resistant carbon fiber composite material according to claim 1, characterized in that: The carbon fiber preform is a plain weave cloth woven from carbon fibers.

3. The high temperature resistant carbon fiber composite material according to claim 1, characterized in that: The inert gas is argon.

4. The high temperature resistant carbon fiber composite material according to claim 2, characterized in that: The slurry is composed of the following components by mass: 60-65 parts of water, 35-40 parts of zirconium phosphate, and 5-8 parts of additives. The preparation steps of the slurry are as follows: Step 1: Take water and put it into the mixing barrel; Step 2: Put the weighed zirconium phosphate into a mixing bucket and stir thoroughly for 30-40 minutes; Step 3: Add 5-8 parts of the weighed additive into the mixing tank, and heat and stir thoroughly for 8-10 minutes; Step 4: Pour out the prepared slurry after cooling.

5. The high temperature resistant carbon fiber composite material according to claim 4, characterized in that: The mass ratio of zirconium phosphate to water in step 2 is 35:

100.

6. The high temperature resistant carbon fiber composite material according to claim 5, characterized in that: The adhesive is composed of the following components by weight: 20-25 parts of butyl acrylate, 20-25 parts of ethyl acetate, 5-10 parts of aluminum oxide, 5-10 parts of silicon micropowder, 10-15 parts of initiator, and 8-10 parts of auxiliary agent; The initiator includes benzoyl peroxide and azobisisobutyronitrile; The specific preparation steps of the adhesive are as follows: Step A1, weigh butyl acrylate and ethyl acetate and put them into a reaction tank; Step A2, adding benzoyl peroxide into a reaction tank to initiate a reaction; Step A3: After a period of reaction, azobisisobutyl cyanide is added to the reaction tank for secondary initiation to obtain a base liquid; Step A4, adding butyl acrylate and ethyl acetate in an amount equal to that in step A1 into the reaction tank again for reaction; Step A5, raising the temperature to 80-90° C., and adding azobisisobutyronitrile dropwise into the reaction tank again; Step A6, after the heat preservation is completed, the remaining ethyl acetate is added to cool down to obtain a finished adhesive product.

7. A method for preparing a high temperature resistant carbon fiber composite material according to claim 6, characterized in that: Here are the steps: Step S1, placing the woven plain fabric in a vacuum furnace and heating it in an inert gas atmosphere; Step S2, after keeping warm for 2 hours, cool to room temperature and take out; Step S3, uniformly coating the prepared slurry and adhesive on the processed carbon fiber plain weave cloth; Step S4, stacking and laying multiple groups of carbon fiber plain weave fabrics coated with slurry and adhesive; Step S5, performing a puncture operation on the carbon fiber plain weave fabric in step S4; Step S6, soaking the composite material in a phosphoric acid solution for 1-2 hours; Step S7, taking out the soaked composite material and heating it to 600° C.; Step S8, placing the composite material in step S7 into a high temperature furnace, heating to 900° C. in an inert gas protective atmosphere, keeping the temperature for 2 hours, and cooling to obtain a high temperature resistant composite material.

8. The method for preparing a high temperature resistant carbon fiber composite material according to claim 7, characterized in that: The coating thickness of the slurry and adhesive in step S3 is 1-10 microns.

9. The method for preparing a high temperature resistant carbon fiber composite material according to claim 7, characterized in that: When the composite material is punctured in step S5, the operating environment is 500-600°C.

10. The method for preparing a high temperature resistant carbon fiber composite material according to claim 7, characterized in that: The inert gas in step S8 is nitrogen.