Oxide ceramic fiber composite aerogel material with infrared shielding and wave absorbing properties and preparation method of oxide ceramic fiber composite aerogel material
By growing SiC nanowires in oxide ceramic fiber aerogel, the problem of sharp increase in thermal conductivity at high temperatures of oxide ceramic fiber aerogel is solved, and it is given wave absorption performance, achieving lightweight and efficient high-temperature heat Protection and wave-absorbing stealth protection, suitable for weapons and equipment.
Patent Information
- Application Number
- CN202410935895.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-12
Smart Images

Figure CN118894731A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic fiber materials, and in particular to an oxide ceramic fiber-based composite aerogel material having both infrared shielding and wave absorbing properties and a preparation method thereof. Background Art
[0002] With the continuous development of aerospace and military technology, supersonic fighters, missiles and other weapons and equipment flying at high Mach numbers must not only face highly harsh thermal environments, but also face the risk of being "shot down as soon as they are discovered" by the enemy's increasingly advanced radar detection devices. An effective way to solve this problem is to use lightweight high-temperature insulation materials and wave-absorbing materials to reduce their weight and improve the flexibility of weapons and equipment while meeting the needs of high-temperature thermal protection and wave-absorbing stealth protection of weapons and equipment.
[0003] Ceramic fiber aerogel has extremely low density and excellent thermal insulation effect due to its extremely high porosity, and is a potential candidate material for high-temperature thermal protection of weapons and equipment. In particular, oxide ceramic fiber aerogels constructed with oxide ceramic fibers such as mullite fiber, alumina fiber, and zirconia fiber, which have low thermal conductivity characteristics at room temperature, have the greatest application potential. However, since oxide ceramic fibers are transparent in the infrared range of ~2.5-7μm, their thermal conductivity increases sharply with increasing temperature, seriously affecting their thermal insulation effect at high temperatures. In addition, since oxide ceramic fiber aerogels do not have wave-absorbing properties, they are currently only used as high-temperature thermal protection materials for weapons and equipment. For the stealth protection of weapons and equipment, only wave-absorbing materials can be used additionally, which will undoubtedly increase the weight of weapons and equipment. Therefore, it is particularly important for the development of weapons and equipment to solve the problem of the sharp increase in thermal conductivity of oxide ceramic fiber aerogels at high temperatures while giving them electromagnetic wave absorption effects. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and to provide an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties and a preparation method thereof; the invention not only solves the problem of a sharp increase in thermal conductivity of oxide ceramic fiber aerogel at high temperatures, but also gives it a certain electromagnetic wave absorption effect, thereby providing high-temperature thermal protection and wave absorbing stealth protection for weapons and equipment at the same time.
[0005] The present invention adopts the following technical solution:
[0006] An oxide ceramic fiber composite aerogel material with both infrared shielding and wave absorbing properties, with oxide ceramic fiber as the basic component unit, SiO2 / C sol as a high-temperature binder, silicon source and carbon source, and a large amount of SiC nanowires grown inside the aerogel through a carbon thermal reduction reaction, forming an oxide-based ceramic fiber composite aerogel material with both infrared shielding and wave absorbing properties.
[0007] A method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties, comprising the following steps:
[0008] Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water, and acid in a molar ratio of 1:4:(16-32):(8-16):(0.01-0.10), and stirring at 25° C.-60° C. for 1-6 hours to obtain a SiO2 / C sol;
[0009] Step 2, ceramic fiber, distilled water, SiO2 / C sol are mixed in a mass ratio of (5-30):1:(0.02-0.15), magnetically stirred at 25°C-60°C for 20-30 minutes, and then placed in an ultrasonic device for 10-20 minutes, and magnetic stirring and ultrasonication are repeated 2-3 times;
[0010] Step 3, placing the fiber dispersion in a refrigerator for 2 to 10 hours, and then placing the sample in a freeze dryer for 24 to 48 hours to obtain a ceramic fiber aerogel body;
[0011] Step 4: placing the ceramic fiber aerogel body in a tubular furnace and performing a high-temperature carbon thermal reduction reaction under the protection of an inert atmosphere to obtain a ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel.
[0012] Furthermore, in step 1, the acid is one of acetic acid, phosphoric acid, nitric acid and hydrochloric acid.
[0013] Furthermore, in step 2, the ceramic fiber is one or more of mullite fiber, zirconia fiber, and alumina fiber; and the length of the ceramic fiber is 15 to 200 μm.
[0014] Furthermore, in step 2, the ceramic fiber dispersion is magnetically stirred for 20 to 30 minutes, and then placed in an ultrasonic device and ultrasonicated at a frequency of 20 to 25 kHz for 10 to 20 minutes; then the ultrasonically treated fiber dispersion is continuously stirred, and this cycle is repeated 2 to 3 times.
[0015] Furthermore, in step 3, the freezing temperature of the refrigerator is -20°C to -80°C.
[0016] Furthermore, in step 3, the vacuum degree of the freeze dryer is always lower than 20 Pa during the freeze drying process.
[0017] Furthermore, in step 4, the heating rate in the tubular furnace is 1-5°C / min, the reaction temperature is 1300°C-1400°C, and the insulation time is 2-6h.
[0018] Furthermore, in step 4, the inert atmosphere is one of nitrogen and argon.
[0019] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects:
[0020] First, the ceramic fiber composite aerogel material prepared by the present invention uses oxide ceramic fiber as the main raw material, and SiO2 / C sol acts as a high-temperature binder, a silicon source and a carbon source respectively, and is prepared by freeze drying combined with a high-temperature carbon thermal reduction reaction; SiC nanowires are grown inside the oxide ceramic fiber composite aerogel material, which can give it infrared shielding performance and electromagnetic wave absorption performance, and at the same time, a large number of SiC nanowires grown are entangled with each other and crisscrossed, which can fill the original macroporous pores of the aerogel, enrich its pore structure, hinder heat transfer and enhance the multiple reflection loss of electromagnetic waves; the prepared aerogel material is light, has low room temperature and high temperature thermal conductivity, and has excellent infrared shielding performance and wave absorption performance, and can be used as a high-temperature thermal protection and wave absorption stealth protection material for supersonic fighters, missiles and other weapons and equipment;
[0021] Second, the SiC nanowires grown inside the ceramic fiber composite aerogel material can improve the infrared shielding performance of the aerogel, which is beneficial to reduce its high-temperature infrared thermal radiation, thereby solving the problem of the sharp increase in thermal conductivity of the oxide ceramic fiber aerogel at high temperatures; and the SiC nanowires themselves have high toughness, which helps to improve the mechanical properties of the oxide ceramic fiber aerogel;
[0022] Third, the infrared transmittance of the oxide ceramic fiber-based composite aerogel material of the present invention is less than 10%, and it has excellent high-temperature heat insulation effect. At the same time, the compressive strength under 10% strain is greater than 0.89MPa; in addition, the wave absorption performance is excellent. When the thickness is 3.6mm, the minimum reflection loss at 7.7GHz reaches -46.2dB, and the effective absorption bandwidth is 2.83GHz;
[0023] Fourthly, the oxide ceramic fiber-based composite aerogel material of the present invention has a simple preparation process and low cost, and is of great significance for the development of integrated materials for high-temperature thermal protection and radar-absorbing stealth protection of weapons and equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a physical picture of the oxide ceramic fiber composite aerogel material prepared in Example 1;
[0025] Figure 2 This is a SEM image of the oxide ceramic fiber composite aerogel material prepared in Example 2 of the present invention;
[0026] Figure 3 This is an infrared transmittance diagram of the oxide ceramic fiber-based composite aerogel material prepared in Example 3 in the wavelength range of 2.5 to 7.0 μm;
[0027] Figure 4This is a graph of electromagnetic wave reflection loss of the oxide ceramic fiber-based composite aerogel material prepared in Example 4. DETAILED DESCRIPTION
[0028] The present invention is further described below through specific implementation modes.
[0029] An oxide ceramic fiber composite aerogel material with both infrared shielding and wave absorbing properties, with oxide ceramic fiber as the basic component unit, SiO2 / C sol as a high-temperature binder, silicon source and carbon source, and a large amount of SiC nanowires grown inside the aerogel through a carbon thermal reduction reaction, forming an oxide-based ceramic fiber composite aerogel material with both infrared shielding and wave absorbing properties.
[0030] The preparation method thereof comprises the following steps:
[0031] Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water, and acid in a molar ratio of 1:4:(16-32):(8-16):(0.01-0.10), and stirring at 25° C.-60° C. for 1-6 hours to obtain a SiO2 / C sol;
[0032] Step 2, mixing the ceramic fiber with distilled water and SiO2 / C sol in a mass ratio of (5-30):1:(0.02-0.15), magnetically stirring at 25°C-60°C for 20-30 minutes, and then placing it in an ultrasonic device for ultrasonication at a frequency of 20-25kHz for 10-20 minutes, and the magnetic stirring and ultrasonication are repeated 2-3 times;
[0033] Step 3, placing the fiber dispersion in a refrigerator at -20°C to -80°C for 2 to 10 hours, then placing the sample in a freeze dryer for 24 to 48 hours, wherein the vacuum degree is always lower than 20 Pa during the freeze drying process, to obtain a ceramic fiber aerogel body;
[0034] Step 4, placing the ceramic fiber aerogel body in a tubular furnace, and performing a high-temperature carbon thermal reduction reaction under the protection of an inert atmosphere to obtain a ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel, wherein the heating rate in the tubular furnace is 1-5°C / min, the reaction temperature is 1300°C-1400°C, and the insulation time is 2-6h.
[0035] Specifically, in step 1, the acid is one of acetic acid, phosphoric acid, nitric acid and hydrochloric acid.
[0036] In step 2, the ceramic fiber is one or more of mullite fiber, zirconia fiber, and alumina fiber; and the length of the ceramic fiber is 15 to 200 μm.
[0037] In step 4, the inert atmosphere is one of nitrogen and argon.
[0038] Example 1
[0039] A method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties, comprising the following steps:
[0040] Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water and phosphoric acid in a molar ratio of 1:4:16:8:0.01, and stirring at 25° C. for 2 h to obtain SiO2 / C sol;
[0041] Step 2, mullite fiber, distilled water, and SiO2 / C sol are mixed in a mass ratio of 8:1:0.03, magnetically stirred at 25°C for 20 minutes, and then placed in an ultrasonic device for 10 minutes, and the magnetic stirring and ultrasonication are cycled twice;
[0042] Step 3, placing the fiber dispersion in a refrigerator for 3 hours, and then placing the sample in a freeze dryer for 24 hours to obtain a ceramic fiber aerogel body;
[0043] Step 4, placing the ceramic fiber aerogel body in a tubular furnace, under the protection of a nitrogen atmosphere, heating the temperature to 1350° C. at a heating rate of 2° C. / min, and keeping the temperature for 2 hours to obtain a mullite-based ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel.
[0044] The material pictures prepared above are as shown in the attached Figure 1 As shown; the thermal conductivity of the fiber at room temperature 25℃ is 0.025W·m -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.053 W·m -1 ·K -1 The infrared transmittance is less than 10% in the band of 2.5 to 7.0 μm; when the thickness is 4.3 mm, the minimum reflection loss at 6.5 GHz reaches -48.2 dB, and the effective absorption bandwidth is 4.62 GHz.
[0045] Example 2
[0046] A method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties, comprising the following steps:
[0047] Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water and hydrochloric acid in a molar ratio of 1:4:20:8:0.03, and stirring at 30° C. for 3 h to obtain SiO2 / C sol;
[0048] Step 2, alumina fiber, distilled water, and SiO2 / C sol were mixed in a mass ratio of 15:1:0.05, magnetically stirred at 30°C for 30 minutes, and then placed in an ultrasonic device for 20 minutes, and magnetic stirring and ultrasonication were repeated 3 times;
[0049] Step 3, placing the fiber dispersion in a refrigerator for 5 hours, and then placing the sample in a freeze dryer for 48 hours to obtain a ceramic fiber aerogel body;
[0050] Step 4, placing the ceramic fiber aerogel body in a tubular furnace, under the protection of argon atmosphere, raising the temperature to 1300° C. at a heating rate of 5° C. / min, and keeping the temperature for 5 hours to obtain an alumina-based ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel.
[0051] The SEM images of the materials prepared above are shown in the attached Figure 2 As shown; the thermal conductivity at room temperature 25℃ is 0.016W·m -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.047 W·m -1 ·K -1 The infrared transmittance is less than 3% in the band of 2.5 to 7.0 μm; when the thickness is 4.9 mm, the minimum reflection loss at 7.2 GHz reaches -52.3 dB, and the effective absorption bandwidth is 3.92 GHz.
[0052] Example 3
[0053] A method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties, comprising the following steps:
[0054] Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water and acetic acid in a molar ratio of 1:4:32:8:0.02, and stirring at 60° C. for 1 h to obtain SiO2 / C sol;
[0055] Step 2, zirconia fiber, distilled water, and SiO2 / C sol are mixed in a mass ratio of 20:1:0.10, magnetically stirred at 60°C for 20 minutes, and then placed in an ultrasonic device for 10 minutes, and the magnetic stirring and ultrasonication are cycled twice;
[0056] Step 3, placing the fiber dispersion in a refrigerator and freezing it for 10 hours, and then placing the sample in a freeze dryer and vacuuming it for 40 hours to obtain a ceramic fiber aerogel body;
[0057] Step 4, placing the ceramic fiber aerogel body in a tubular furnace, under the protection of a nitrogen atmosphere, heating the temperature to 1360° C. at a heating rate of 3° C. / min, and keeping the temperature for 3 hours to obtain a zirconia-based ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel.
[0058] The thermal conductivity of the prepared material at room temperature 25°C is 0.025 W·m -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.061 W·m -1 ·K -1 , the infrared transmittance is less than 6% in the wavelength range of 2.5 to 7.0 μm. Figure 3 As shown; when the thickness is 3.3mm, its minimum reflection loss at 6.5GHz reaches -43.1dB, and the effective absorption bandwidth is 4.75GHz.
[0059] Example 4
[0060] A method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties, comprising the following steps:
[0061] Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water and nitric acid in a molar ratio of 1:4:16:8:0.05, and stirring at 30° C. for 6 h to obtain SiO2 / C sol;
[0062] Step 2, mullite fiber, distilled water, and SiO2 / C sol are mixed in a mass ratio of 30:1:0.15, magnetically stirred at 30°C for 30 minutes, and then placed in an ultrasonic device for 20 minutes, and the magnetic stirring and ultrasonication are cycled for 3 times;
[0063] Step 3, placing the fiber dispersion in a refrigerator and freezing it for 10 hours, and then placing the sample in a freeze dryer and vacuuming it for 48 hours to obtain a ceramic fiber aerogel body;
[0064] Step 4, placing the ceramic fiber aerogel body in a tubular furnace, under the protection of argon atmosphere, heating the temperature to 1400° C. at a rate of 2° C. / min, and keeping the temperature for 2 hours to obtain a mullite-based ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel.
[0065] The thermal conductivity of the material prepared above is 0.013 W·m at room temperature 25°C. -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.041 W·m -1 ·K -1 , the infrared transmittance is less than 1% in the band of 2.5-7.0μm; when the thickness is 3.6mm, the minimum reflection loss at 7.7GHz is -46.2dB, the effective absorption bandwidth is 2.83GHz, and the electromagnetic wave reflection loss is Figure 4 shown.
[0066] In summary, the infrared transmittance of the oxide ceramic fiber-based composite aerogel material of the present invention is less than 10%, and it has excellent high-temperature heat insulation effect. At the same time, the compressive strength under 10% strain is greater than 0.89MPa; in addition, the wave absorbing performance is excellent. When the thickness is 3.6mm, the minimum reflection loss at 7.7GHz reaches -46.2dB, and the effective absorption bandwidth is 2.83GHz; its preparation process is simple and the cost is low, which is of great significance to the development of integrated materials for high-temperature thermal protection and wave absorbing stealth protection of weapons and equipment.
[0067] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the application scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. An oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties, characterized in that: With oxide ceramic fiber as the basic component unit, SiO2 / C sol as high-temperature binder, silicon source and carbon source, a large number of SiC nanowires are grown inside the aerogel through carbon thermal reduction reaction, forming an oxide-based ceramic fiber composite aerogel material with both infrared shielding and wave absorbing properties.
2. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 1, characterized in that: The following steps are involved: Step 1, mixing tetraethyl orthosilicate, glucose, ethanol, distilled water, and acid in a molar ratio of 1:4:(16-32):(8-16):(0.01-0.10), and stirring at 25° C.-60° C. for 1-6 hours to obtain a SiO2 / C sol; Step 2, ceramic fiber, distilled water, SiO2 / C sol are mixed in a mass ratio of (5-30):1:(0.02-0.15), magnetically stirred at 25°C-60°C for 20-30 minutes, and then placed in an ultrasonic device for 10-20 minutes, and magnetic stirring and ultrasonication are repeated 2-3 times; Step 3, placing the fiber dispersion in a refrigerator for 2 to 10 hours, and then placing the sample in a freeze dryer for 24 to 48 hours to obtain a ceramic fiber aerogel body; Step 4: placing the ceramic fiber aerogel body in a tubular furnace and performing a high-temperature carbon thermal reduction reaction under the protection of an inert atmosphere to obtain a ceramic fiber composite aerogel material with SiC nanowires grown inside the aerogel.
3. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 1, the acid is one of acetic acid, phosphoric acid, nitric acid and hydrochloric acid.
4. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 2, the ceramic fiber is one or more of mullite fiber, zirconia fiber, and alumina fiber; and the length of the ceramic fiber is 15 to 200 μm.
5. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 2, the ceramic fiber dispersion is magnetically stirred for 20 to 30 minutes, and then placed in an ultrasonic device and ultrasonicated at a frequency of 20 to 25 kHz for 10 to 20 minutes; then the ultrasonically treated fiber dispersion is continuously stirred, and this cycle is repeated 2 to 3 times.
6. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 3, the freezing temperature of the refrigerator is -20°C to -80°C.
7. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 3, the vacuum degree of the freeze dryer is always lower than 20 Pa during the freeze drying process.
8. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 4, the heating rate in the tubular furnace is 1-5°C / min, the reaction temperature is 1300°C-1400°C, and the holding time is 2-6h.
9. The method for preparing an oxide ceramic fiber composite aerogel material having both infrared shielding and wave absorbing properties according to claim 2, characterized in that: In step 4, the inert atmosphere is one of nitrogen and argon.
Citation Information
Patent Citations
Heat-insulation stealthy high-temperature-resistant gas inlet duct and production method thereof
CN107804041A
Infrared shielding coating modified fiber reinforced aerogel thermal insulation material and preparation method thereof
CN110698101A
Preparation method of flexible high-temperature-resistant silicon carbide aerogel composite thermal insulation material
CN115611632A
Silicon dioxide aerogel heat shield composite material and manufacturing method therefor