Framework type light ceramsite proppant and preparation method and sintering device thereof
By designing the skeleton structure and cladding layer in the ceram proppant and combining with a special sintering device, the problems of strength and flow-guiding ability of the ceram proppant when reducing the apparent density are solved, and the lightweightness of the ceram proppant is achieved. High strength and good flow diversion effect.
Patent Information
- Application Number
- CN202411072767.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing ceram proppants are difficult to maintain high strength and diversion capacity while reducing the apparent density, which easily leads to an increase in the breakage rate and affects the diversion effect.
Using a skeleton-type lightweight ceramic proppant, by forming through holes and particles on the ceramic skeleton and using a petroleum resin coating, combined with a specific sintering device design, including a powder sprinkler device to spray ceramic powder, to form multi-point contact and Increase the diversion gap.
The lightweight, high strength and good flow diversion effect of the ceram proppant are achieved, the crushing rate is reduced, the flow diversion capacity and migration distance are improved, and the support effect in the oil and gas mining process is enhanced.
Smart Images

Figure CN118894733A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramsite proppants, and in particular to a skeleton-type lightweight ceramsite proppant and a preparation method and a sintering device thereof. Background Art
[0002] In the process of oil and natural gas extraction, many construction processes use proppants to fill cracks to make the cracks have higher conductivity, thereby establishing effective production channels. This greatly improves the conductivity of the original oil and gas reservoir. Therefore, the performance of the proppant plays a vital role in its conductivity and resistance to crack closure during the production process.
[0003] In the prior art, many scholars have conducted relevant research on the composition and preparation process of proppants to improve their various properties, including low density, high strength, high conductivity, etc. Liu Chunting verified through simulation in "Numerical Simulation of Proppant Transport and Settling Behavior in Hydraulic Fractures" (Daqing Petroleum Geology and Development, Vol. 37, No. 5, October 2018) that the smaller the proppant particle size or density, the greater the proppant migration distance in the hydraulic fracture. In order to achieve better support effects, relevant research has also been conducted, such as proppant graded injection, displacement fluid injection, and the use of a variety of stability fluids to assist injection (CN 109072065B), etc. However, the simplest way is to inject the proppant after grading and mixing. When the large-particle proppant has a lower apparent density and the small-particle proppant has a higher apparent density, a better support effect can be achieved through grading.
[0004] Therefore, a large-particle ceramsite proppant with a smaller apparent density is needed. However, the method of reducing the apparent density in the prior art is usually to select a material with a smaller density and increase the pore size inside the ceramsite. While reducing the apparent density, the strength of the proppant is also reduced, the crushing rate is increased, and the conductivity is easily reduced. Summary of the invention
[0005] The above technical problems have not been solved. The present invention provides a skeleton-type lightweight expanded clay proppant and a preparation method and a sintering device thereof, which are mainly used for expanded clay proppant with a particle size range of 20-40 meshes. The produced proppant has the characteristics of being light, high-strength, able to carry sand and liquid farther and having good diversion effect.
[0006] In order to achieve the above object, the technical solution used in the present invention is:
[0007] A skeleton-type lightweight ceramsite proppant comprises a ceramic skeleton and an oil-soluble coating layer coated on the outside of the ceramic skeleton; the ceramic skeleton is provided with through holes and particles, and the particles are formed on the outer surface of the ceramic skeleton.
[0008] Furthermore, the ceramic skeleton with through holes accounts for 35%-45% of the total ceramic skeleton.
[0009] Furthermore, the coating layer is petroleum resin, and the coating layer covers the through holes on the ceramic skeleton.
[0010] A method for preparing a skeleton-type lightweight ceramsite proppant comprises the following steps:
[0011] Step S1: batching and homogenizing: taking bauxite powder, kaolin powder, potassium feldspar powder, pyrolusite powder, bamboo fiber powder and barite powder, stirring and homogenizing to obtain a homogenized material;
[0012] Step S2: granulation; adding the homogenized material obtained in step S1 and a small amount of polyvinyl alcohol aqueous solution into a strong mixing granulator for granulation to obtain a granular material;
[0013] Step S3: pre-sintering; the pellets obtained in step S2 are kept at 65-75°C in a heating box for 3-6 hours, then heated to 700°C at a rate of 5-8°C / min under oxygen-rich conditions, kept warm for more than 30 minutes, crushed and sieved to obtain a pellet;
[0014] Step S4: sintering; the ball blank obtained in step S3 is heated to 1400°C ± 10°C at a rate of 3°C / min under oxygen-rich conditions, and kept warm for 1 hour, and sieved twice after cooling to obtain a ceramic skeleton; during the sintering process, the bamboo fiber powder is oxidized and burned to form through holes;
[0015] Step S5: coating: using a coating layer material to coat the outer surface of the ceramic skeleton obtained in step S4 to obtain a skeleton-type lightweight ceramsite proppant;
[0016] In the process of heat preservation, ceramic powder is sprayed onto the surface of the ball blank to form particles.
[0017] Compared with the prior art, the proppant produced by the present invention has through holes with a diameter of dozens to several tens of microns, which reduces the apparent density of the proppant and improves the flow conductivity. During the sintering process of the ball blank, ceramic powder is sprayed on the surface of the ball blank. The ceramic powder has a high melting point and can reduce the agglomeration of the ceramic skeleton. It can also remain outside the ceramic skeleton to form raised particles, thereby increasing the gaps between the proppants and forming multi-point contacts between the ceramic skeletons to a certain extent, thereby increasing the compressive strength of the proppant and making it less likely to break.
[0018] Furthermore, in step S1, the homogenized material includes, by mass, 35-45 parts of bauxite, 40-55 parts of kaolin, 4-10 parts of potassium feldspar, 2-3 parts of pyrolusite, 2-3 parts of bamboo fiber powder, and 0.5-1.5 parts of barite.
[0019] Furthermore, the preparation method of the bamboo fiber powder is as follows: 20-40 mesh bamboo powder is screened twice through a 40 mesh sieve, the remaining part is taken, soaked and rubbed in a 5% NaOH aqueous solution at 85-90° C. for 60-90 minutes, rinsed with clean water and dried to obtain the powder.
[0020] After chemical treatment, the bamboo powder is sieved to remove short fibers and select more suitable bamboo fiber powder, which is suitable for use as a pore-forming agent for a proppant.
[0021] Furthermore, in step S1, bauxite, kaolin, feldspar and pyrolusite are all ground into powders with a particle size of less than 300 meshes.
[0022] Furthermore, in the step S4, the ceramic powder is a powder obtained by crushing the unqualified products after the secondary screening in the step S4, and the particle size of the ceramic powder is 150-200 meshes.
[0023] This particle size range not only satisfies the purpose of spacing the proppants and reducing adhesion, but also can form raised particles on the surface of the proppants to increase the contact points between the proppants.
[0024] Furthermore, in step S5, the thickness of the coating layer on the outer surface of the ceramic skeleton is 10-12 μm.
[0025] Petroleum resin can reduce the apparent density of proppants, allowing them to migrate farther. In the early stages of formation closure, it can increase the contact area between proppants and increase conductivity during oil and gas production.
[0026] A sintering device for a skeleton-type lightweight ceramsite proppant comprises a rotary kiln having a kiln head, a kiln body and a kiln tail, and also comprises a powder sprinkling device, wherein the powder sprinkling device extends from the kiln head into the rotary kiln and sprays ceramic powder into the rotary kiln.
[0027] The only difference between the device for sintering proppants of the present invention and the prior art is that a powder sprinkling device not found in the prior art is provided. The powder sprinkling device sprays ceramic powder onto the ball blank during the heat preservation process, making the proppants of the present invention significantly different from other proppants in appearance and effect.
[0028] Furthermore, the powder sprinkling device comprises a ventilation pipe and a screw conveyor, the ventilation pipe is coaxially sleeved outside the discharge pipe of the screw conveyor, and the length of the ventilation pipe extending into the rotary kiln is greater than the length of the discharge pipe of the screw conveyor extending into the rotary kiln.
[0029] The screw conveyor can quantitatively convey, and an air duct is arranged outside the screw conveyor. On the one hand, the air duct can disperse the heavy crystal powder and have good contact with the proppant in the rotary kiln. On the other hand, the ventilation of the air duct can prevent the high temperature inside the rotary kiln from affecting the screw conveyor.
[0030] Beneficial Effects
[0031] 1. The skeleton-type lightweight ceramsite proppant of the present invention has through holes, and the protruding particles on the surface can make the contact between adjacent proppants no longer a single-point contact, but can produce a multi-point contact state, which limits the relative slippage of the proppants on the one hand, and can also increase the gap between the proppants on the other hand, further improving the flow conductivity. The coating layer is a petroleum resin, which closes the holes on the surface of the proppant when the proppant is formed, reduces the apparent density, and in the initial stage of sedimentation after the proppant is injected, the surface of the petroleum resin is smooth, which can make the adjacent proppants have a certain position adjustment slip state when contacting each other, increase the contact points between adjacent proppants, and in the process of formation closure and oil and gas production, the petroleum resin gradually softens and dissolves, so that the through holes formed by the bamboo fiber powder are opened, the flow conductivity of the support system is increased, and the yield is improved.
[0032] 2. In the preparation method of the skeleton-type lightweight expanded clay proppant of the present invention, bamboo fiber powder is processed and made to form through holes with smaller diameters, and during the sintering process, the bamboo fiber is oxidized and burned to form through holes. Compared with the through hole forming in the prior art, it is more convenient and quicker, and at the same time does not excessively affect the strength of the proppant, reducing the breakage rate of the proppant.
[0033] 3. In the method for preparing the skeleton-type lightweight ceramsite proppant of the present invention, the particles protruding on the surface of the proppant are formed relatively uniformly, and mutual adhesion between the proppants can be suppressed during the sintering process.
[0034] 4. The sintering device of the skeleton-type lightweight ceramsite proppant of the present invention is not much different from the sintering device in the prior art, the cost of adding components for modification is low, and the modified sintering device can simultaneously produce the proppant in the prior art and the proppant of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic diagram of a structure in which a plurality of skeleton-type lightweight ceramsite proppants of the present invention are adjacent to each other;
[0036] Figure 2 It is a process flow chart of the preparation method of the skeleton-type lightweight ceramsite proppant of the present invention;
[0037] Figure 3 It is a cross-sectional view of a sintering device for a skeleton-type lightweight ceramsite proppant according to the present invention.
[0038] The numbers in the attached figure are: 1, ceramic skeleton; 2, through hole; 3, particles; 4, coating layer; 5, rotary kiln; 6, kiln head cover; 7, cooling belt; 8, exhaust duct; 9, gas burner; 10, powder sprinkling device; 11, ventilation pipe; 12, screw conveyor. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0040] like Figure 1 As shown, a skeleton-type lightweight ceramsite proppant comprises a ceramic skeleton 1 and an oil-soluble coating layer 4 coated outside the ceramic skeleton; the ceramic skeleton is provided with through holes 2 (such as Figure 1 The shaded part) and the particles 3 are formed on the outer surface of the ceramic skeleton 1.
[0041] The coating layer 4 is oil-soluble petroleum resin, and the coating layer 4 covers and seals the through hole.
[0042] The coating layer 4 is oil-soluble and seals the pores on the surface of the proppant when the proppant is formed. The "pores" here include the open pores on the surface of the ceramic skeleton and the through holes 2 that penetrate the ceramic skeleton. These pores are sealed, which can reduce the apparent density, so that the 20 / 40 mesh proppant of the present invention has a lower apparent density than other proppants. After being graded with proppants of other particle sizes, it can be transported farther with the sand liquid and has a stronger supporting effect on the cracks. In the initial stage of sedimentation after the proppant is injected, the coating layer surface is smooth, which can make the adjacent proppants have a certain position adjustment slip state when they contact each other (here refers to when one proppant settles to contact with another proppant, Because the surface of the coating layer 4 is smooth, the settled proppant particles can form a relative sliding state (rotation or other forms of relative sliding) relative to the proppant below to a certain extent, increasing the contact points between adjacent proppants and making the stacking state between the proppants more stable. During the formation closure and oil and gas production process, the petroleum resin gradually softens and dissolves, so that the through holes formed by the bamboo fiber powder are opened, the conductivity of the support system is increased, and the output is improved. At the same time, there are particles 3 on the ceramic surface, and these particles 3 can be "stuffed" between two adjacent proppants, so that there are multiple points of contact between the two adjacent proppants, increasing the proppant conductivity gap of the proppant or increasing the contact area between the proppants, and improving the compressive strength.
[0043] like Figure 2 As shown, a method for preparing a skeleton-type lightweight ceramsite proppant is used to prepare the above-mentioned skeleton-type lightweight ceramsite proppant, comprising the following steps:
[0044] Step S1: batching and homogenizing: taking bauxite powder, kaolin powder, potassium feldspar powder, pyrolusite powder, bamboo fiber powder and barite powder, stirring and homogenizing to obtain a homogenized material;
[0045] Step S2: granulation; adding the homogenized material obtained in step S1 and a small amount of polyvinyl alcohol aqueous solution into a strong mixing granulator for granulation to obtain a granular material;
[0046] Step S3: pre-sintering; the pellets obtained in step S2 are kept at 65-75°C in a heating box for 3-6 hours, then heated to 700°C at a rate of 5-8°C / min under oxygen-rich conditions, kept warm for more than 30 minutes, crushed and sieved to obtain a pellet;
[0047] Step S4: sintering; heating the ball blank obtained in step S3 to 1400°C ± 10°C at a rate of 3°C / min under oxygen-rich conditions, and keeping the temperature for 1 hour, cooling, and sieving twice to obtain a ceramic skeleton 1;
[0048] Step S5: coating; using a coating layer material to coat the outer surface of the ceramic skeleton 1 obtained in step S4, thereby obtaining a skeleton-type lightweight ceramsite proppant;
[0049] During the heat preservation process, ceramic powder is sprayed onto the surface of the ball blank to form particles 3.
[0050] In the step S1, the homogenized material includes, by mass, 35-45 parts of bauxite, 40-55 parts of kaolin, 4-10 parts of potassium feldspar, 2-3 parts of pyrolusite, 2-3 parts of bamboo fiber powder, and 0.5-1.5 parts of barite.
[0051] Among them, bauxite and kaolin are the main components of the ceramic skeleton 1. The ceramic skeleton 1 forms a lightweight ceramic material containing 34%-42% alumina under the above ratio. Potash feldspar is mainly used to reduce the sintering temperature. The bamboo fiber is ablated at high temperature during the molding process. The ceramic powder can form particles 3 on the surface of the proppant, reducing the adhesion between adjacent proppants during the insulation process.
[0052] The preparation method of the bamboo fiber powder is as follows: 20-40 mesh bamboo powder is screened twice through a 40 mesh sieve, the remaining part is taken, soaked and rubbed in a 5% NaOH aqueous solution at 85-90° C. for 60-90 minutes, rinsed with clean water and dried to obtain the bamboo fiber powder.
[0053] Bamboo powder is a powder obtained by crushing the debris generated when mechanically processing bamboo products. The powder has not been subjected to any chemical treatment, so the original chemical composition of bamboo is completely retained. In addition to bamboo fiber powder, there are some other substances, but we only use bamboo fiber powder, so further treatment is required to retain only bamboo fiber powder. After bamboo powder is soaked and rubbed in 5% NaOH aqueous solution at 85-90°C for 60-90 minutes, most of the lignin, fat, pectin and other impurities are removed, thereby forming a fiber bundle. The diameter (width direction) of the fiber bundle is 40μm-90μm on average, while the length usually does not change much, still 350μm-830μm. At this time, the bamboo fiber powder is suitable for being used as a pore-forming agent for a proppant. The main purpose of screening after chemical treatment is to remove too short fibers. The present invention strives to form through holes on the proppant, rather than closed holes, because too short fibers cannot form through holes.
[0054] In step S1, bauxite, kaolin, feldspar and pyrolusite are ground into powders with a particle size of less than 300 meshes.
[0055] Generally speaking, the smaller the particles, the easier it is to ball and sinter, and the better the sintering effect. However, considering all factors, 300 mesh can achieve better ball and sintering effects, and the cost is lower.
[0056] In the step S4, the ceramic powder is a powder obtained by crushing the unqualified products after the secondary screening in the step S4, the particle size of the ceramic powder is 150-200 meshes, and the spraying amount is 1-2kg / ton of pellets.
[0057] The particle size of the ceramic powder is about one tenth to one fifth of the diameter of the proppant. The refractory strength of the ceramic powder is greatly improved after the sintering process. It is not easy to melt after being sprayed into the sintering device, thereby separating adjacent ball blanks and reducing adhesion. During the insulation process, the ceramic powder combines with the liquid in the ball blank to form particles 3 on the surface of the proppant.
[0058] In step S5, the thickness of the coating layer 4 on the outer surface of the ceramic skeleton 1 is 10-12 μm.
[0059] Petroleum resin will not be destroyed at room temperature and in water. It can close the open pores on the surface of the proppant, reduce the apparent density of the proppant, and make the proppant more convenient to be transported by the sand-carrying fluid. After being mixed with small-particle proppant, it has a longer migration distance. In the early stage of formation closure, it can make better relative position adjustment between proppants and increase the contact area between proppants. The coating layer will gradually soften and dissolve under the action of high temperature and oil and gas, exposing the through holes formed by bamboo fiber powder and increasing the conductivity.
[0060] like Figure 3 As shown, a sintering device for a skeleton-type lightweight ceramsite proppant comprises a rotary kiln 5, wherein the rotary kiln 5 has a kiln head, a kiln body and a kiln tail. A kiln head hood 6 is provided at the kiln head of the rotary kiln 5, and the kiln head hood 6 is connected to a cooling belt 7 and an exhaust duct 8. A gas burner 9 is provided at the end of the kiln head hood 6, and the gas burner 9 penetrates the kiln head hood 6 and extends into the kiln head of the rotary kiln 5. The device also comprises a powder sprinkling device 10, which penetrates the kiln head hood 6 and extends from the kiln head into the rotary kiln 5, and sprays ceramic powder into the rotary kiln 5.
[0061] The only difference between the device for sintering proppants of the present invention and the prior art is that a powder sprinkling device 10 not found in the prior art is provided. The powder sprinkling device 10 sprays ceramic powder onto the ball blank during the sintering process, making the proppants of the present invention significantly different from other proppants in appearance and effect.
[0062] The powder sprinkling device 10 includes a ventilation pipe 11 and a screw conveyor 12. The ventilation pipe 11 is coaxially sleeved on the outside of the discharge pipe of the screw conveyor 12. The length of the ventilation pipe 11 extending into the rotary kiln 5 is greater than the length of the discharge pipe of the screw conveyor 12 extending into the rotary kiln 5. The ventilation pipe 11 is fixedly connected to the kiln head cover 6.
[0063] The screw conveyor 12 can carry out quantitative metering transportation. A ventilation pipe 11 is arranged outside the screw conveyor 12. On the one hand, the ventilation pipe 11 can disperse the heavy crystal powder and make it contact well with the proppant in the rotary kiln 5. On the other hand, ventilation of the ventilation pipe 11 can prevent the high temperature inside the rotary kiln 5 from affecting the screw conveyor 12.
[0064] Embodiment 1
[0065] The raw materials of the ceramic skeleton 1 include, by mass, 45 parts of bauxite, 43 parts of kaolin, 7.5 parts of potassium feldspar, 2 parts of pyrolusite, 2 parts of bamboo fiber powder, and 0.5 parts of barite.
[0066] Embodiment 2
[0067] The raw materials of the ceramic skeleton 1 include, by mass, 35 parts of bauxite, 54.5 parts of kaolin, 4 parts of potassium feldspar, 3 parts of pyrolusite, 2.5 parts of bamboo fiber powder, and 1 part of barite.
[0068] Embodiment 3
[0069] The raw materials of the ceramic skeleton 1 include, by mass, 40.7 parts of bauxite, 43 parts of kaolin, 10 parts of potassium feldspar, 2 parts of pyrolusite, 2.8 parts of bamboo fiber powder, and 1.5 parts of barite.
[0070] Embodiment 4
[0071] The raw materials of the ceramic skeleton 1 include, by mass, 40 parts of bauxite, 50 parts of kaolin, 4 parts of potassium feldspar, 3 parts of pyrolusite, 2 parts of bamboo fiber powder, and 1 part of barite.
[0072] The above four embodiments are all produced by the preparation method of the skeleton-type lightweight ceramsite proppant of the present invention, and the obtained product performance is as follows:
[0073]
[0074] The proportion of ceramic skeletons with through holes in the above table is relatively low, on the one hand because there is no bamboo fiber powder inside the particles during granulation, and on the other hand because the through holes are closed by particles during sintering.
[0075] Since the proppant of the present invention has a special structure, the effect of the coating layer is that the apparent density is different when injected and when used, and the conductivity of the proppant system can be improved while ensuring the crushing rate.
[0076] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
Claims
1. A skeleton-type lightweight ceramsite proppant, It is characterized in that It comprises a ceramic skeleton (1) and an oil-soluble coating layer (4) coated on the outside of the ceramic skeleton; the ceramic skeleton is provided with through holes (2) and particles (3), and the particles (3) are formed on the outer surface of the ceramic skeleton (1).
2. The skeleton-type lightweight ceramsite proppant according to claim 1, It is characterized in that The coating layer (4) is petroleum resin, and the coating layer (4) seals the through holes (2) on the ceramic skeleton (1).
3. A method for preparing a skeleton-type lightweight ceramsite proppant, used for preparing the skeleton-type lightweight ceramsite proppant according to any one of claims 1 to 2, It is characterized in that The following steps are involved: Step S1: batching and homogenizing: taking bauxite powder, kaolin powder, potassium feldspar powder, pyrolusite powder, bamboo fiber powder and barite powder, stirring and homogenizing to obtain a homogenized material; Step S2: granulation; adding the homogenized material obtained in step S1 and a small amount of polyvinyl alcohol aqueous solution into a strong mixing granulator for granulation to obtain a granular material; Step S3: pre-sintering; the pellets obtained in step S2 are kept at 65-75°C in a heating box for 3-6 hours, then heated to 700°C at a rate of 5-8°C / min under oxygen-rich conditions, kept warm for more than 30 minutes, crushed and sieved to obtain a pellet; Step S4: sintering; heating the ball blank obtained in step S3 to 1400°C ± 10°C at a rate of 3°C / min under oxygen-rich conditions, and keeping the temperature for 1 hour, cooling, and sieving twice to obtain a ceramic skeleton (1); Step S5: coating; using a coating layer material to coat the outer surface of the ceramic skeleton (1) obtained in step S4, thereby obtaining a skeleton-type lightweight ceramsite proppant; In the process of heat preservation, ceramic powder is sprayed onto the surface of the ball blank to form particles (3).
4. The method for preparing the skeleton-type lightweight ceramsite proppant according to claim 3, It is characterized in that In the step S1, the homogenized material includes, by mass, 35-45 parts of bauxite, 40-55 parts of kaolin, 4-10 parts of potassium feldspar, 2-3 parts of pyrolusite, 2-3 parts of bamboo fiber powder, and 0.5-1.5 parts of barite.
5. The method for preparing the skeleton-type lightweight ceramsite proppant according to claim 4, It is characterized in that The preparation method of the bamboo fiber powder is as follows: 20-40 mesh bamboo powder is screened twice through a 40 mesh sieve, the remaining part is taken, soaked and rubbed in a 5% NaOH aqueous solution at 85-90° C. for 60-90 minutes, rinsed with clean water and dried to obtain the bamboo fiber powder.
6. The method for preparing the skeleton-type lightweight ceramsite proppant according to claim 4, It is characterized in that In the step S1, bauxite, kaolin, feldspar and pyrolusite are ground into powders with a particle size of less than 300 meshes.
7. The method for preparing the skeleton-type lightweight ceramsite proppant according to claim 3, It is characterized in that In the step S4, the ceramic powder is obtained by crushing the unqualified products after the secondary screening in the step S4, and the particle size of the ceramic powder is 150-200 meshes.
8. A sintering device for a skeleton-type lightweight ceramsite proppant, used for preparing the skeleton-type lightweight ceramsite proppant according to any one of claims 1 to 2, comprising a rotary kiln (5), wherein the rotary kiln (5) has a kiln head, a kiln body and a kiln tail, It is characterized in that It also comprises a powder sprinkling device (10), wherein the powder sprinkling device (10) extends from the kiln head into the rotary kiln (5) and sprays ceramic powder into the rotary kiln (5).
9. The sintering device of the skeleton-type lightweight ceramsite proppant according to claim 8, It is characterized in that The powder sprinkling device (10) comprises a ventilation pipe (11) and a screw conveyor (12); the ventilation pipe (11) is coaxially sleeved on the outside of a discharge pipe of the screw conveyor (12); the length of the ventilation pipe (11) extending into the rotary kiln (5) is greater than the length of the discharge pipe of the screw conveyor (12) extending into the rotary kiln (5).
Citation Information
Patent Citations
Methods to enhance flow conductivity through post-fracture channel formation
CN109072065B
High-strength ceramsite propping agent and production method thereof
CN101914374A
Low-density oil fracturing propping agent and preparation method thereof
CN102786921A
Preparation method of low-density high-intensity film covering ceramic support agent
CN106278349A
Method for extracting wood fibers from branches and straws
CN111995768A