Self-photosensitive catalytic platinum (II) complex material as well as preparation method and application thereof
By introducing specific ligands into the platinum (II) complex for ring metallization and optimizing its structure, the problem of insufficient light absorption capacity and stability of the platinum (II) complex in the photocatalytic reduction of carbon dioxide reaction is solved, and more efficient photocatalytic reduction of carbon dioxide reaction.
Patent Information
- Application Number
- CN202410932338.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing platinum (II) complexes have insufficient light absorption capacity and unstable structural in the photocatalytic reduction carbon dioxide reaction, resulting in unsatisfactory catalytic effect.
By introducing ligands of 2-(2-thienyl)pyridine and 4,4'-dimethyltriphenyl groups, cyclic metallization reaction with divalent platinum ions, a self-photosensitive catalyzed platinum (II) complex is formed. Its structure is optimized to enhance light absorption capacity and stability, so that the Pt center is exposed and catalytically active in the reaction.
It significantly improves the light absorption capacity and structural stability of the platinum (II) complex under visible light, improves the efficiency of photocatalytic reduction of carbon dioxide, and becomes an efficient catalyst that combines "photosensitive + catalytic" dual properties.
Smart Images

Figure CN118894889A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic materials and relates to a self-photosensitive catalytic platinum (II) complex material and a preparation method and application thereof. Background Art
[0002] Due to modern industrialization, humans have emitted a large amount of carbon dioxide into the atmosphere, and these emissions have exacerbated global climate change. The increase in carbon dioxide emissions has intensified the greenhouse effect, leading to an increase in the overall temperature of the earth, which has had a serious impact on global biodiversity, agricultural production and human health. In addition, rising temperatures have also accelerated the rise in sea levels, posing a huge threat to coastal communities and ecosystems. Therefore, reducing and controlling carbon dioxide emissions is an urgent task to protect the earth and the future of mankind. The use of artificially constructed photocatalytic reduction of carbon dioxide systems to reduce carbon dioxide to substances with high utilization value such as carbon monoxide and formic acid is of great significance for alleviating environmental problems, solving the energy shortage crisis, and achieving the goals of "carbon peak" and "carbon neutrality".
[0003] At present, various types of complexes have been developed in the application field of metal complexes, and certain effects have been achieved in the catalytic reduction of carbon dioxide. For example, metal complexes based on cobalt, iron, copper, nickel, rhenium, ruthenium, iridium, palladium, etc. have shown certain catalytic ability or photosensitivity in the photocatalytic reduction of carbon dioxide. Platinum metal is a widely used catalyst; however, there are few reports on the application of its complexes in homogeneous photocatalytic reduction of carbon dioxide systems. In addition, traditional platinum (II) complexes have a simple structure and are easy to be rapidly degraded during the catalytic reduction reaction. Rapid inactivation, absorption range in the visible light absorption spectrum The absorption intensity is poor, so when When this type of platinum (II) complex is used in fields involving light energy conversion such as photocatalytic reactions, the effect is often not ideal. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the first purpose of the present invention is to provide a self-photosensitive catalytic platinum (II) complex material, which has a stronger light absorption ability under visible light and an enhanced overall structural stability. The structure of one side of the main ligand is stable and does not decompose, and the ligand on the other side of the structure is free and falls off during the reaction, exposing the Pt center. The Pt center catalytically reduces CO2 to products such as CO, making it a highly efficient self-photosensitive catalyst with dual properties of "photosensitive + catalytic".
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned self-photocatalytic platinum (II) complex material.
[0006] The third object of the present invention is to provide an application of the above self-photocatalytic platinum (II) complex material.
[0007] The first object of the present invention can be achieved by adopting the following technical solutions:
[0008] A self-photosensitive catalytic platinum (II) complex material having a structure shown in Formula I:
[0009]
[0010] The second object of the present invention can be achieved by adopting the following technical solutions:
[0011] A method for preparing a self-photosensitive catalytic platinum (II) complex material comprises the following steps:
[0012] Step S1, reacting a ligand of the structure shown in Formula II with chloroplatinate to prepare a platinum (II) dimer of the structure shown in Formula III;
[0013] Step S2, depolymerizing the platinum (II) dimer prepared in step S1 in a DMSO solution to obtain the self-photosensitive catalytic platinum (II) complex material;
[0014] The structure shown in formula II is:
[0015]
[0016] The structure shown in formula III is:
[0017]
[0018] Furthermore, step S1 is carried out in a solvent, wherein the solvent is a mixed solvent of ethylene glycol ethyl ether and water, and the volume ratio of ethylene glycol ethyl ether to water is (1-5):1.
[0019] Furthermore, the molar ratio of the ligand to chloroplatinate is (1-1.2):1.
[0020] Furthermore, the reaction conditions are: 70-90° C. for 3-48 hours under an inert gas atmosphere.
[0021] Furthermore, in step S2, the reaction conditions are: reflux reaction for 1-5 hours under an inert gas atmosphere.
[0022] Furthermore, in step S1, after the reaction is completed, a solid-liquid separation and purification process is performed: the reaction liquid is cooled to room temperature, water is added, and filtered to obtain a crude product of platinum (II) dimer; and the crude product of platinum (II) dimer is washed with one or more of dichloromethane, ether, n-hexane and ethanol in sequence.
[0023] Furthermore, in step S2, after the reaction is completed, a solid-liquid separation and purification process is performed: The reaction solution was cooled to room temperature Add water to filter and obtain the crude product, dissolve it in dichloromethane, and add n-hexane toRecrystallization is performed to obtain the self-photosensitive catalytic platinum (II) complex material.
[0024] Furthermore, the chloroplatinate is sodium chloroplatinate or potassium chloroplatinate and hydrates thereof.
[0025] Furthermore, the ligand of the structure shown in Formula II is prepared via the following preparation route:
[0026]
[0027] Furthermore, the compound of the structure shown in formula IV is prepared via the following preparation route:
[0028]
[0029] The third object of the present invention can be achieved by adopting the following technical solutions:
[0030] The self-photosensitive platinum (II) complex material is used as a self-photosensitive photocatalytic reaction catalyst, and the self-photosensitive photocatalytic reaction catalyst is used for photocatalytic reduction of carbon dioxide.
[0031] Furthermore, the self-photosensitive photocatalytic reaction catalyst and the synergistic catalyst are used together for photocatalytic reduction of carbon dioxide; the synergistic catalyst is [Co(TPA)ClO4]ClO4.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The present invention provides a self-photosensitive catalytic platinum (II) complex material, which is obtained by a cyclometallation reaction between a ligand containing 2-(2-thienyl) pyridine and 4,4′-dimethyltriphenylamine groups and a divalent platinum ion; a large conjugated group and an electron-donating group are introduced to optimize the structure, so that the platinum complex has a stronger light absorption ability under visible light, and its overall structural stability is enhanced, so that the structure of one side of the main ligand is stable and does not decompose; the ligand on the other side of the structure is freed and dropped during the reaction, so that the Pt center is exposed and has catalytic activity, and thus it is a highly potential high-efficiency self-photosensitive catalyst with dual properties of "photosensitive + catalytic".
[0034] 2. The present invention provides a method for preparing a self-photosensitive catalytic platinum (II) complex material, wherein a ligand containing a 2-(2-thienyl) pyridine group undergoes a cyclometalation reaction with a divalent platinum ion to obtain a dimer, and then a depolymerization reaction is carried out in a solvent to obtain a platinum (II) complex. The reaction can occur at a relatively low temperature under an inert gas, and harsh reaction conditions are not required.
[0035] 3. The application of a self-photosensitive catalytic platinum (II) complex material of the present invention can absorb more blue light in the photocatalytic reduction reaction of carbon dioxide under 460nm light irradiation, and has a high efficiency in converting photon energy into chemical reaction energy, and has better photosensitivity than traditional platinum (II) complexes. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is the nuclear magnetic hydrogen spectrum of the self-photosensitive catalytic platinum (II) complex material (I) of the present invention;
[0037] Figure 2 The infrared spectrum of the self-photosensitive catalytic platinum (II) complex material (I) of the present invention;
[0038] Figure 3 The absorption spectrum of the self-photosensitive catalytic platinum (II) complex material (I) of the present invention is picture;
[0039] Figure 4 The single crystal structure diagram of the self-photosensitive catalytic platinum (II) complex material (I) of the present invention;
[0040] Figure 5 The molecular structure diagram of the self-photosensitive catalytic platinum (II) complex material (I) of the present invention. DETAILED DESCRIPTION
[0041] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only partial embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0042] Existing platinum (II) complexes, such as Pt-ppy-Cl-DMSO platinum (II) complexes using traditional organic ligand 2-phenylpyridine (ppy);
[0043]
[0044] The light absorption range and light absorption intensity in the visible light absorption spectrum are poor. Therefore, when this type of platinum (II) complex is used in the field of photocatalytic reaction and other light energy conversion, the effect is often not ideal. And due to its simple structure, it is easy to be quickly deactivated in the catalytic reduction reaction, which is not conducive to the efficient operation of the system.
[0045] Therefore, the present invention provides a self-photosensitive catalytic platinum (II) complex material; having a structure shown in formula I, such as Figure 5 As shown:
[0046]
[0047] A self-photosensitive catalytic platinum (II) complex material of the present invention has a structure shown in Formula I, wherein the ligand is a 2-(2-thienyl) pyridine group, and a 4,4'-dimethyltriphenylamine group is connected to the 2-position of the group, and the benzene ring on the ppy ligand is replaced by the thiophene group, and the ligand 4,4'-dimethyltriphenylamine is connected to the thiophene group, and then the N on the pyridine and a carbon atom on the thiophene form a five-membered ring with platinum. By introducing a large conjugated group and an electron-donating group for structural optimization, it exhibits a stronger light absorption ability under visible light, and enhances its overall structural stability, so that the structure of one side of the main ligand is stable and does not decompose, and the Pt material itself has catalytic activity for carbon dioxide, and the ligand on the other side of the structure is free and dropped during the reaction process, so that the Pt center is exposed, and the Pt center catalytically reduces CO2 to products such as CO, making it a highly potential "photosensitive + catalytic" dual-property high-efficiency self-photosensitive catalyst.
[0048] A method for preparing a self-photosensitive catalytic platinum (II) complex material comprises the following steps:
[0049] Step S1, reacting a ligand of the structure shown in Formula II with chloroplatinate to prepare a platinum (II) dimer of the structure shown in Formula III;
[0050] Step S2, depolymerizing the platinum (II) dimer prepared in step S1 in a DMSO solution to obtain the self-photosensitive catalytic platinum (II) complex material;
[0051] The structure shown in formula II is:
[0052]
[0053] The structure shown in formula III is:
[0054]
[0055] The ligand of the structure shown in formula II undergoes a cyclometalation reaction with the divalent platinum ion of chloroplatinate to obtain a platinum dimer of the structure shown in formula III, and the self-photosensitive catalytic platinum (II) complex material is obtained after depolymerization in an organic solvent. The ligand of the structure shown in formula II undergoes a cyclometalation reaction with the divalent platinum ion of chloroplatinate at the four-position carbon of the thiophene ring and the N atom of the pyridine ring, and forms a five-membered ring after cyclometalation with platinum.
[0056] As one embodiment, step S1 is performed in a solvent, wherein the solvent is a mixed solvent of ethylene glycol ethyl ether and water, wherein the volume ratio of ethylene glycol ethyl ether to water is (1-5):1; preferably, the volume ratio of ethylene glycol ethyl ether to water is 3:1. The water is preferably deionized water.
[0057] As one embodiment, the molar ratio of the ligand to the chloroplatinate is (1-1.2): 1. A slight excess of the ligand can fully form platinum dimers, which is convenient for subsequent separation and purification. Preferably, the molar ratio of the ligand to the chloroplatinate is 1.05:1.
[0058] As one embodiment, the reaction conditions are: 70-90° C. for 3-48 hours under an inert gas atmosphere. The inert gas atmosphere may be nitrogen or argon. A reaction temperature of 70-90° C. can ensure efficient reaction.
[0059] As one embodiment, in step S2, the reaction conditions are: reflux reaction for 1-5 hours under an inert gas atmosphere. Step S2 is a depolymerization process of platinum dimer.
[0060] As one embodiment, in step S1, after the reaction is completed, a solid-liquid separation and purification process is performed: the reaction liquid is cooled to room temperature, water is added, and filtered to obtain a crude product of platinum (II) dimer; and the crude product of platinum (II) dimer is washed with one or more of dichloromethane, ether, n-hexane and ethanol in sequence. Washing with an organic reagent can remove unreacted ligands.
[0061] As one embodiment, in step S2, after the reaction is completed, a solid-liquid separation and purification process is performed: the reaction liquid is cooled to room temperature, water is added, filtered to obtain a crude product, dissolved in dichloromethane, and recrystallized in n-hexane to obtain the self-photosensitive catalytic platinum (II) complex material.
[0062] As one embodiment thereof, the chloroplatinate is sodium chloroplatinate or potassium chloroplatinate and hydrates thereof. Sodium chloroplatinate or potassium chloroplatinate has good solubility, and the sodium chloride or potassium chloride obtained after the reaction has good water solubility and is easily dissolved in water for removal.
[0063] As one embodiment, the ligand of the structure shown in Formula II is prepared via the following preparation route:
[0064]
[0065] 2-(2-thienyl)pyridine is used as a starting material, and a halogen atom, especially a bromine atom, is connected to the 5 position of the thiophene ring to replace the benzene ring on the ppy ligand; pinacol borate is connected to the para position of a benzene ring of the ligand 4,4′-dimethyltriphenylamine as a reactive group, and the bromine atom on the thiophene group is replaced by a coupling reaction to obtain a ligand of the structure shown in formula II, and thienylpyridine undergoes a cyclometalation reaction with a divalent platinum ion.
[0066] As one embodiment, 2-bromothiophene pyridine is dissolved in an organic solvent, and NBS is slowly added thereto for reaction; after the reaction is completed, 5-bromo-2-thiophene pyridine is obtained after purification.
[0067] In this embodiment, the molar ratio of 2-bromothiophene pyridine to NBS is 1; (1-1.2); the organic solvent is preferably chloroform; the reaction is protected from light, and the reaction time is 3-12 hours. The purification is silica gel column chromatography; n-hexane is used as the eluent; the reaction yield reaches more than 72%.
[0068] As one embodiment, 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine and 5-bromo-2-thiophenepyridine are reacted in a solvent under a zero-valent palladium catalyst system to obtain a ligand with a structure shown in Formula II.
[0069] In this embodiment, the molar ratio of 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine to 5-bromo-2-thienylpyridine is 1:(1-1.2); the zero-valent palladium catalytic system is a mixture of tetrakistriphenylphosphine palladium and potassium carbonate; the molar ratio of triphenylphosphine palladium and potassium carbonate is 0.05:(1.5-3); the amount of tetrakistriphenylphosphine palladium added is 0.02-0.1 equivalents of 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine; the solvent is a mixed solvent of toluene / ethanol / water, wherein the volume ratio of toluene / ethanol / water is 7:1:2.
[0070] The reaction conditions are 80-100° C. for 3-24 h under an inert gas atmosphere.
[0071] The separation and purification steps after the reaction are as follows: after the reaction stops, the solvent is removed, and the organic layer is extracted and dried with ethyl acetate and saturated brine, and the concentrated organic layer is purified by column chromatography, and the eluent ratio is petroleum ether / ethyl acetate / dichloromethane (20 / 1 / 1, v / v / v).
[0072] As one embodiment, the compound of the structure shown in formula IV is prepared via the following preparation route:
[0073]
[0074] 4-Bromo-4′,4″-dimethyltriphenylamine reacts with bis-pinacol diboron, potassium acetate and [1,1′-bis(diphenylphosphino)ferrocene] dichloropalladium(II) in a solvent to obtain a compound 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine with a structure shown in formula IV.
[0075] In this embodiment, the molar ratio of 4-bromo-4′,4″-dimethyltriphenylamine, bis-pinacolyl diboron, potassium acetate, and [1,1′-bis(diphenylphosphino)ferrocene]dichloropalladium(II) is 1:(2-3):(1-6):(0.01-0.1); and the solvent is 1,4-dioxane.
[0076] The reaction conditions are 80-110° C. for 3-24 h under an inert gas atmosphere.
[0077] The separation and purification steps of the reaction are as follows: the reaction solution is extracted and dried with dichloromethane and water to obtain an organic layer, and then purified by column chromatography, with the eluent being n-hexane / ethyl acetate (20 / 1, v / v).
[0078] The self-photosensitive platinum (II) complex material of the present invention is used as a self-photosensitive photocatalytic reaction catalyst, and the self-photosensitive photocatalytic reaction catalyst is used for photocatalytic reduction of carbon dioxide.
[0079] As one embodiment, the self-photosensitive photocatalytic reaction catalyst and the synergistic catalyst are used together for photocatalytic reduction of carbon dioxide; the synergistic catalyst is [Co(TPA)ClO4]ClO4.
[0080] The following is a further description with reference to specific embodiments.
[0081] Example 1
[0082] 1) Synthesis of 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine (IV): 4-bromo-4′,4″-dimethyltriphenylamine (0.3522 g, 1 mmol), bis-pinacol diboron (0.6355 g, 2.5 mmol), potassium acetate (0.2944 g, 3 mmol), [1,1′-bis(diphenylphosphino)ferrocene] dichloropalladium (II) (0.0424 g, 0.058 mmol) were placed in a 100 mL single-necked flask, and 50 mL of solvent 1,4-dioxane was added. The mixture was reacted at 100° C. for 16 h under the protection of nitrogen. The reaction solution was extracted and dried with dichloromethane and water to obtain an organic layer, which was purified by column chromatography. The eluent was n-hexane / ethyl acetate (20 / 1, v / v) to obtain 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine. The yield was 35%.
[0083] 2) Synthesis of 5-bromo-2-thiophenepyridine (V): Weigh 2-bromothiophenepyridine (0.1630 g, 1 mmol) and dissolve it in 50 mL of chloroform. Slowly add NBS (0.1869 g, 1.05 mmol) and react overnight in the dark. After the reaction, concentrate the reaction solution and add an appropriate amount of silica gel. Then, dry-sample the solution with n-hexane as the eluent. After purification, 5-bromo-2-thiophenepyridine is obtained with a yield of 72%.
[0084] 3) Synthesis of ligand (II): 4-boronic acid pinacol ester-4′,4″-dimethyltriphenylamine (0.1198 g, 0.3 mmol), 5-bromo-2-thiophene pyridine (0.0792 g, 0.33 mmol), tetrakistriphenylphosphine palladium (0.0173 g, 0.015 mmol), potassium carbonate (0.0829 g, 0.6 mmol) were weighed in a 100 mL single-necked flask, 30 mL of solvent toluene / ethanol / deionized water (7 / 1 / 2, v / v / v) was added, and the mixture was reacted at 100° C. under nitrogen protection overnight; after the reaction stopped, the solvent was removed by vortexing, and the organic layer was extracted and dried with ethyl acetate and saturated brine to obtain the organic layer, and the organic layer was concentrated and purified by column chromatography, and the eluent ratio was petroleum ether / ethyl acetate / dichloromethane (20 / 1 / 1, v / v / v) to obtain ligand II, with a yield of 67%;
[0085] 4) Synthesis of self-photocatalytic platinum (II) complex material (I): weigh ligand II (0.0865 g, 0.2 mmol), potassium tetrachloroplatinate (0.0789 g, 0.19 mmol), 12 mL of ethylene glycol ether / deionized water (3 / 1, v / v) in a 50 mL single-necked flask, and react at 80 ° C for 10 h under nitrogen protection; the reaction solution is cooled to room temperature, 30 mL of deionized water is added, and filtered to obtain a crude product platinum (II) dimer, and then a small amount of dichloromethane, ether, n-hexane and ethanol and other solvents are used to wash away impurities in the crude product to obtain product III, with a yield of 90%;
[0086] Weigh III, dissolve it with 3 mL of dimethyl sulfoxide (DMSO), and reflux for 2 h under the protection of nitrogen. After the reaction solution is cooled to room temperature, deionized water is added to precipitate and filter to obtain a crude product, which is then dissolved with dichloromethane and collected. Most of the dichloromethane is removed by a rotary evaporator, and n-hexane is added for recrystallization several times to obtain a self-photosensitive catalytic platinum (II) complex material (I), named Pt-Dmtpa-thiopy-Cl-DMSO, with a yield of 45%.
[0087] Compound characterization:
[0088] (1) The NMR data of Pt-Dmtpa-thiopy-Cl-DMSO is: 1 H NMR(400MHz,Chloroform-d)δ9.27(d,J=6.1Hz,1H),7.82-7.63(m,2H),7.48(d,J= 8.6Hz,2H),7.32(d,J=8.0Hz,1H),7.11-6.93(m,10H),3.62(s,6H),2.32(s,6H), see Figure 1 .
[0089] (2) The infrared spectrum of Pt-Dmtpa-thiopy-Cl-DMSO is shown in Figure 2 shown.
[0090] from Figure 2 It can be seen that 3021.66cm -1 The absorption peak at 3087.74 cm is the unsaturated CH stretching vibration in the benzene ring. -1 The peak at 2917.22 cm corresponds to the CH stretching vibration of the methyl group. -1 The peak at 1600-1467.85cm should be attributed to the CH stretching vibration on the benzene ring. -1 The peak between is the skeleton vibration peak of the benzene ring, 1322.91cm -1 CN stretching vibration 1600-1401.77cm -1 It should be attributed to the C=C symmetric stretching vibration and C=C asymmetric stretching vibration on the thiophene ring, 1288.8 cm -1 The peak at 1154.42 cm corresponds to the in-plane bending vibration of CH on the thiophene ring. -1 The peak at 819.89 cm should be attributed to the stretching vibration of the SO bond. -1 The peak at 762.95 cm-1 should be caused by the out-of-plane bending vibration of CH on the thiophene ring. -1 The peak at is the out-of-plane deformation vibration of CH on the aromatic ring.
[0091] (3) The absorption spectra of Pt-Dmtpa-thiopy-Cl-DMSO and Pt-ppy-Cl-DMSO platinum (II) complexes are shown in Figure 3 As shown;
[0092] In the study of photocatalytic reduction of carbon dioxide, researchers generally use blue light from 400nm to 460nm as the light source. When the traditional platinum (II) complex Pt-ppy-Cl-DMSO is used as a photosensitizer, its visible light absorption capacity is insufficient, especially in the range of 400nm to 460nm, it has almost no absorption capacity. Figure 3 As shown in the figure, the absorption intensity of the UV-visible absorption spectrum of Pt-ppy-Cl-DMSO between 400nm and 460nm is very small, and the absorption peak is mainly distributed between 200-400nm. -5mol / L), the absorption intensity of Pt-Dmtpa-thiopy-Cl-DMSO between 400nm and 460nm is as high as 0.0989 (at 456nm) and as low as 0.0531 (at 407nm), and the light absorption capacity of Pt-Dmtpa-thiopy-Cl-DMSO is much stronger than that of Pt-ppy-Cl-DMSO. Therefore, in the photocatalytic reduction of carbon dioxide under 400 to 460nm blue light irradiation, Pt-Dmtpa-thiopy-Cl-DMSO has better light absorption efficiency.
[0093] (4) The single crystal structure of Pt-Dmtpa-thiopy-Cl-DMSO is shown in the figure below. Figure 4 The single crystal data are shown in Table 1; the bond lengths and bond angles of the characteristic bonds are shown in Table 2.
[0094] Table 1 X-ray crystal data of Pt-Dmtpa-thiopy-Cl-DMSO
[0095]
[0096] a R1=Σ||Fo|-|Fc|| / Σ|Fo|.wR2={Σ[w(Fo 2 -Fc 2 ) 2 ] / Σ[w(Fo 2 ) 2 ]} 1 / 2 .
[0097] b GoF=[(Σw|Fo|-|Fc|) 2 / (Nobs-Nparam)] 1 / 2 .
[0098] Table 2 Bond lengths and bond angles of characteristic bonds of Pt-Dmtpa-thiopy-Cl-DMSO.
[0099]
[0100] Photocatalytic performance test
[0101] 1) Pt-Dmtpa-thiopy-Cl-DMSO stock solution was prepared using DMA (N,N′-dimethylacetamide) solvent as the photosensitizer in the reaction system, and 1,3-dimethyl-2-phenyl-2,3-dihydro-1H-benzimidazole (BIH) was used as the electron sacrifice in the reaction system. A 10 mL ground-mouth thick-walled round-bottom test tube was used as the reaction container in the experiment, and the reaction system in the photocatalytic experiment was 2 mL in total.
[0102] (2) Place a stirring magnet in the test tube, and add a photosensitizer, an electron sacrificial agent, and a solvent. In the system, the concentration of Pt-Dmtpa-thiopy-Cl-DMSO is 0.4mM, 0.1M BIH, and DMA (N,N′-dimethylacetamide) is used as the solvent. Plug the tube with a rubber stopper and seal the bottleneck with a sealing film. Use a long needle to pass carbon dioxide into the solution in the test tube for 50 minutes to ensure that the carbon dioxide reaches saturation in the solution, and then seal the rubber stopper with electrical glue.
[0103] (3) Finally, the aerated test tube was stirred under a magnetic stirrer and irradiated with a 460nm visible blue LED lamp at a reaction temperature of 25°C. After 24 hours of illumination, the carbon monoxide content in the test tube was detected by gas chromatography, and the formic acid content in the test tube was detected by ion chromatography until the reaction was completed. The total reaction time was 120 hours. The conversion data was obtained according to the standard curve equation for quantitative detection of the product established by the analytical instrument used, as shown in Table 3. Table 3 Application of Pt-Dmtpa-thiopy-Cl-DMSO as a self-photosensitive catalyst in the homogeneous photocatalytic reduction of carbon dioxide
[0104]
[0105] As can be seen from Table 3, in the presence of 0.4 mM Pt-Dmtpa-thiopy-Cl-DMSO of the present application, the total light reaction time is 120 h, the CO production reaches 29.3 umol, the selectivity is as high as 94%, and the TON is 37. In the control group 2 without adding 0.4 mM Pt-Dmtpa-thiopy-Cl-DMSO of the present application, the light reaction is also 120 h, and no CO is produced, indicating that carbon dioxide is not reduced to CO.
[0106] (4) Add mature catalysts to the system and co-catalyze with Pt-Dmtpa-thiopy-Cl-DMSO. Add 0.0125mM [Co(TPA)ClO4]ClO4, use 460nm visible blue LED light for irradiation, and the reaction temperature is 25°C. After every 24h of irradiation, the product of the reaction system is detected until the reaction is completed. The total reaction time is 120h. The results are shown in Table 4:
[0107] Table 4 Pt-Dmtpa-thiopy-Cl-DMSO as a self-photosensitized catalyst and [Co(TPA)ClO4]ClO4 catalyst were used in homogeneous photocatalytic reduction of carbon dioxide
[0108]
[0109] From the data in Table 3, it can be seen that when 0.0125 mM [Co(TPA)ClO4]ClO4 is added as a co-catalyst in the reaction system, the CO content reaches 49.1 umol, which is almost twice that when [Co(TPA)ClO4]ClO4 is not added. The selectivity still reaches 93%, but the TON has reached 1962, which is much higher than the effect when [Co(TPA)ClO4]ClO4 is not added.
[0110] When there was only [Co(TPA)ClO4]ClO4 in the control group 4, no CO was produced, indicating that simply containing [Co(TPA)ClO4]ClO4 could not convert carbon dioxide into CO; this also means that [Co(TPA)ClO4]ClO4 was used in conjunction with the Pt-Dmtpa-thiopy-Cl-DMSO of the present application, and the synergistic and efficient catalysis significantly improved the efficiency of the reaction system.
[0111] In summary, the self-photosensitive catalytic platinum (II) complex material (I) of the present application, based on the ligand 2-(5-bromo-2-thienyl) pyridine, uses a thiophene group connected to a bromine atom to replace the benzene ring, and then uses a ligand 4,4′-dimethyltriphenylamine to replace the bromine atom on the thiophene group to form a new ligand, and undergoes a cyclometallation reaction with a divalent platinum ion to obtain a self-photosensitive catalytic platinum (II) complex material (I); a large conjugated group and an electron-donating group are introduced for structural optimization, showing a stronger light absorption ability under visible light, and enhancing its overall structural stability, so that the structure of one side of the main ligand is stable and does not decompose; the ligand on the other side of the structure is freed and dropped during the reaction, exposing the Pt center, and the Pt material itself has catalytic activity for carbon dioxide, and the Pt center catalytically reduces CO2 to products such as CO, becoming a highly potential "photosensitive + catalytic" dual-property high-efficiency self-photosensitive catalyst.
[0112] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A self-photocatalytic platinum (II) complex material, characterized in that: It has the structure shown in formula I:
2. The method for preparing a self-photosensitive catalytic platinum (II) complex material according to claim 1, characterized in that: The following steps are involved: Step S1, reacting a ligand of the structure shown in Formula II with chloroplatinate to prepare a platinum (II) dimer of the structure shown in Formula III; Step S2, depolymerizing the platinum (II) dimer prepared in step S1 in a DMSO solution to obtain the self-photosensitive catalytic platinum (II) complex material; The structure shown in formula II is: The structure shown in formula III is:
3. The method for preparing the self-photosensitive catalytic platinum (II) complex material according to claim 2, characterized in that: Step S1 is carried out in a solvent, wherein the solvent is a mixed solvent of ethylene glycol ethyl ether and water, and the volume ratio of ethylene glycol ethyl ether to water is (1-5):1; The molar ratio of the ligand to chloroplatinate is (1-1.2):1; The reaction conditions are: 70-90°C for 3-48h under an inert gas atmosphere.
4. The method for preparing the self-photosensitive catalytic platinum (II) complex material according to claim 2, characterized in that: In step S2, the reaction conditions are: reflux reaction for 1-5 hours under an inert gas atmosphere.
5. The method for preparing the self-photosensitive catalytic platinum (II) complex material according to claim 2, characterized in that: In step S1, after the reaction is completed, a solid-liquid separation and purification process is performed: the reaction liquid is cooled to room temperature, water is added, and filtered to obtain a crude product of platinum (II) dimer; and the crude product of platinum (II) dimer is washed with one or more of dichloromethane, ether, n-hexane and ethanol in sequence; In step S2, after the reaction is completed, a solid-liquid separation and purification process is performed: the reaction solution is cooled to room temperature, water is added, filtered to obtain a crude product, dissolved in dichloromethane, and recrystallized with n-hexane to obtain the self-photosensitive catalytic platinum (II) complex material.
6. The method for preparing the self-photosensitive catalytic platinum (II) complex material according to claim 2, characterized in that: The chloroplatinate is sodium chloroplatinate or potassium chloroplatinate and hydrates thereof.
7. The method for preparing the self-photosensitive catalytic platinum (II) complex material according to claim 2, characterized in that: The ligand of the structure shown in formula II is prepared via the following preparation route:
8. The method for preparing the self-photosensitive catalytic platinum (II) complex material according to claim 7, characterized in that: The compound of the structure shown in formula IV is prepared via the following preparation route:
9. Use of the self-photosensitive platinum (II) complex material according to any one of claims 1 to 8 as a self-photosensitive photocatalytic reaction catalyst, characterized in that: The self-photosensitive photocatalytic reaction catalyst is used for photocatalytic reduction of carbon dioxide.
10. The use according to claim 9, characterized in that: The self-photosensitive photocatalytic reaction catalyst and the synergistic catalyst are used together for photocatalytic reduction of carbon dioxide; the synergistic catalyst is [Co(TPA)ClO4]ClO4.
Citation Information
Patent Citations
Polycyclic phenylpyridine iridium complexes and derivatives thereof for OLEDs
CN105555792A
Bromine atom modified blue light absorption enhanced iridium (III) complex and preparation method thereof
CN113801170A
Method for constructing stable organic biradical molecules in air based on lock effect
CN116410235A
Organic electroluminescent element, display and lighting device
JP2006120762A
Metal complex and organic letroluminescent devices
US20050147843A1