Polymer and preparation method thereof, binder, positive pole piece, secondary battery and electric device

By developing a polymer containing specific repeating structural units as a binder, the problem of insufficient mechanical strength and flexibility of the positive electrode sheet in the prior art has been solved, and the performance of the secondary battery is significantly improved, especially during processing and use. Stability in the process.

CN118894956APending Publication Date: 2024-11-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310498058.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The oil-based binder used in existing lithium-ion batteries is costly and cannot meet the increasing requirements, resulting in insufficient mechanical strength and flexibility of the positive electrode sheet of the secondary battery, making it difficult to meet the needs of complex stresses.

Method used

A polymer has been developed, including specific first, second and third repeat structural units, to improve the overall performance of the polymer through synergistic effects, making it suitable as a binder for the positive electrode sheet, enhancing mechanical strength and flexibility. , reduce the probability of breakage and peeling of the material layer.

Benefits of technology

As a binder, the polymer significantly improves the mechanical strength and flexibility of the positive electrode sheet, reduces the risk of breakage and peeling during processing and use, and improves the overall performance of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894956A_ABST
    Figure CN118894956A_ABST
Patent Text Reader

Abstract

The invention relates to a polymer and a preparation method thereof, a binder, a positive pole piece, a secondary battery and an electric device, the polymer comprises a first repetitive structure unit shown as a formula I, a second repetitive structure unit shown as a formula II and a third repetitive structure unit shown as a formula III, the average polymerization degree of the first repetitive structure unit is 50-120, and the average polymerization degree of the third repetitive structure unit is 50-120. The average polymerization degree of the second repeating structure unit is 25-60, and the average polymerization degree of the third repeating structure unit is 25-60. The polymer disclosed by the invention has better cohesiveness, so that the pole piece containing the polymer has proper mechanical strength, and the flexibility of the pole piece containing the polymer can also be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery technology, and specifically relates to a polymer and a preparation method thereof, a binder, a positive electrode sheet, a secondary battery and an electrical device. Background Art

[0002] In recent years, with the widespread application of secondary batteries, such as sodium-ion batteries, their performance has received more and more attention, and as a result, there is an increasing demand for binders in the active layers of the electrode, such as the positive electrode active material layer.

[0003] PVDF is the most commonly used oily binder in the lithium-ion battery industry. It is expensive, which increases the cost of battery production, and its performance cannot meet the increasingly high requirements. Therefore, the comprehensive performance of the binder still needs to be improved. Summary of the invention

[0004] The purpose of the present application is to provide a polymer and a preparation method thereof, which can be used as a binder for a positive electrode plate to improve the mechanical strength and flexibility of the positive electrode plate; the present application also aims to provide a binder, a positive electrode plate, a secondary battery and an electrical device that can achieve the beneficial effects of the polymer.

[0005] In a first aspect, an embodiment of the present application provides a polymer, comprising a first repeating structural unit shown in formula I, a second repeating structural unit shown in formula II, and a third repeating structural unit shown in formula III,

[0006]

[0007] Wherein, R1 includes an optionally substituted amide group, -R4COORc, -R6SO3R d , 3-6 membered N-containing heterocyclic group, -R7-PO(OR e )2, wherein R4 is empty or includes C1-C11 alkylene, Rc includes H, any one of optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations; R6 is empty or includes C1-C11 alkylene, R d Including H, any one of optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations; R7 is empty or includes any one of C1-C11 alkylene, -O-, and C1-C11 alkyleneoxy; R e independently include any one of H, optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations;

[0008] R2 includes any one of C4-C12 ester group, C4-C12 alkoxy acyl group, C4-C12 acyl amine group, C3-C8 cycloalkyl group, and C2-C8 heterocycloalkyl group;

[0009] R3 includes any one of C3-C12 alkyl, C3-C12 alkyl alkenyl, C4-C12 alkoxyalkyl, and substituted or unsubstituted C1-C6 acylamino;

[0010] The average polymerization degree of the first repeating structural unit is 50-120, the average polymerization degree of the second repeating structural unit is 25-60, and the average polymerization degree of the third repeating structural unit is 25-60.

[0011] In the polymer according to the embodiment of the present application, the repeating structural units with different structures give the polymer good comprehensive properties through synergistic effects, making it suitable for use as a binder in the positive electrode sheet. In the polymer, the first repeating structural unit has a group with strong polarity. On the one hand, such a group makes the polymer molecules have a strong interaction, which can improve the cohesive strength of the polymer. On the other hand, it has a strong affinity for the current collector material and the positive electrode active material such as aluminum, so that the polymer has good wettability and adhesion to the current collector material and the positive electrode active material; the second repeating structural unit has any one of an ester group, an alkoxy acyl group, an acylamine group, a cycloalkyl group and a heterocycloalkyl group with a certain number of carbon atoms, and such a group makes the polymer have good wettability and adhesion to weak polar materials; the third repeating structural unit has a soft side chain with an appropriate carbon chain length, which can increase the free volume of the polymer and give the polymer good flexibility.

[0012] The polymer of the present application is used for the active material layer of the electrode. The polymer can provide a certain strength and flexibility for the active material layer in the positive electrode, and the polymer can provide a certain strength and flexibility for the active material layer in the positive electrode, so that the probability of breakage and / or peeling of the active material layer of the prepared electrode during processing and use is greatly reduced.

[0013] In any embodiment of the present application, the polymer is a random copolymer. The random copolymer has good processing performance and bonding performance.

[0014] In any embodiment of the present application, the polymer comprises a branched polymer chain. The branched polymer chain can further improve the flexibility of the above polymer and can increase the solubility of the polymer, thereby improving the processing performance of using the polymer for the preparation of the positive electrode sheet.

[0015] In any embodiment of the present application, R1 comprises the structural formula: -CONH(CH2) x SO3H sulfonyl substituted amide group, -(CH2) yCOOH, one or more of the 5-membered lactam rings, wherein x is an integer of 1 to 5; y is an integer of 0 to 12. Such groups, on the one hand, allow for stronger interactions between polymer molecules, which can improve the cohesive strength of the polymer, and on the other hand, have a stronger affinity for current collector materials such as aluminum and positive electrode active materials, thereby allowing the polymer to have good wettability and adhesion to current collector materials and positive electrode active materials.

[0016] In addition, the 5-membered lactam ring has a similar group to the pyrrolidone group of NMP in the slurry system of N-methylpyrrolidone (NMP), which can enhance the solubility of the polymer in the slurry and improve the degree of interaction between the positive electrode active material and the polymer, which is beneficial to improving the cohesion and flexibility of the positive electrode sheet.

[0017] In any embodiment of the present application, R2 includes -COO(CH2) p CH3, wherein p is an integer from 2 to 10, or -OCO(CH2) q CH3, wherein q is an integer of 2 to 10. The ester group or alkoxy acyl group having a certain number of carbon atoms is a group with weak polarity, which can improve the good wettability and adhesion of the polymer to weak polar materials.

[0018] In any embodiment of the present application, R3 includes -(CH2) p CH=CH2、-CH2O(CH2) q CH3, -CH2O(CH2) q One or more of CH3; wherein p is an integer of 2 to 10, and q is an integer of 4 to 10. The above groups have soft side chains with appropriate carbon chain lengths, which can increase the free volume of the polymer and give the polymer good flexibility. When the positive electrode sheet containing the polymer is subjected to complex stresses during preparation and cycling, the electrode sheet containing the polymer has a certain flexibility, which can reduce the probability of surface fracture or cracking of the positive electrode sheet during processing and use.

[0019] In any embodiment of the present application, the molar ratio of the first repeating structural unit, the second repeating structural unit and the third repeating structural unit in the polymer is 100: (20.5-120): (20.5-120). The molar ratio of the first repeating structural unit, the second repeating structural unit and the third repeating structural unit in the polymer is within the above range, which can increase the functionality of the polymer having the above structural unit and improve its adhesion; at the same time, the spatial conformational change of the polymer having the above structural unit can be enhanced, so that the electrode containing the polymer has a certain mechanical strength and flexibility. For example, when the polymer is used in the positive active material layer, the probability of fracture or cracking of the surface active material layer of the electrode during processing and use can be reduced.

[0020] In any embodiment of the present application, the molar ratio of the first repeating structural unit to the third repeating structural unit is 5: (2-12). When the molar ratio of the first repeating structural unit to the third repeating structural unit in the polymer is within the above range, the active material layer of the pole piece, especially the positive electrode active material layer of the positive pole piece, has both good mechanical strength and excellent flexibility, which can avoid the probability of the active material layer of the pole piece breaking or cracking during winding or folding.

[0021] In any embodiment of the present application, the weight average molecular weight of the polymer is 500000-1800000, and can be optionally 80000-1200000. When the weight average molecular weight of the polymer is within the above range, the molecular chain of the polymer has a certain length, which can increase the change of the molecular configuration of the polymer and increase the active functional groups, thereby improving the bonding performance of the polymer and improving the flexibility of the electrode containing the polymer.

[0022] In any embodiment of the present application, the polymer has a structure shown in any one of H1-H19:

[0023]

[0024]

[0025]

[0026] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers. According to the embodiment of the present application, the electrode piece containing the compound having any of the above structures can make the electrode piece have suitable mechanical strength and better flexibility.

[0027] In a second aspect, the present application provides a method for preparing a polymer, comprising:

[0028] Mixing a monomer corresponding to the first repeating structural unit, a monomer corresponding to the second repeating structural unit, and a monomer corresponding to the third repeating structural unit with a free radical initiator in a dispersion medium to obtain a reaction mixture;

[0029] Initiate a free radical initiator to polymerize the monomer to obtain a polymer according to any one of claims 1 to 10; wherein the monomer corresponding to the first repeating structural unit has a structural formula shown in Formula Ia, R1CH=CH2(Ia), R1 includes an optionally substituted amide group; -R4COORc, wherein R4 is empty or includes a C1-C11 alkylene group, and Rc includes H, an optionally substituted ammonium ion, an alkali metal cation; -R6SO3R d , wherein R6 is empty or includes C1-C11 alkylene, Rd Including H, optionally substituted ammonium ion, alkali metal cation; 3-5 membered N-containing heterocyclic group; -R7-PO3(R e )2, R7 is empty or includes C1-C11 alkylene, -O-, C1-C11 alkyleneoxy, R e independently comprising H, optionally substituted ammonium ions, alkali metal cations;

[0030] The monomer corresponding to the second repeating structural unit has the structural formula shown in formula II-a, R2CH=CH2(II-a),

[0031] R2 includes any one of C4-C12 ester group, C4-C12 alkoxy acyl group, C4-C12 acyl amine group, C3-C8 cycloalkyl group, and C2-C8 heterocycloalkyl group;

[0032] The monomer corresponding to the third repeating structural unit has the structural formula shown in formula III-a, R3CH=CH2(III-a),

[0033] R3 includes any one of C3-C12 alkyl, C3-C12 alkylalkenyl, C4-C12 alkoxyalkyl, and substituted or unsubstituted C1-C6 acylamino.

[0034] The preparation method of the present application has a simple process and does not require multiple complex reactions, and can be synthesized in one step. In the prepared polymer, the first repeating structural unit has a group with strong polarity. On the one hand, such a group allows a strong interaction between polymer molecules, which can improve the cohesive strength of the polymer. On the other hand, it has a strong affinity for current collector materials and positive electrode active materials such as aluminum, so that the polymer has good wettability and adhesion to current collector materials and positive electrode active materials; the second repeating structural unit has an ester group or alkoxy acyl group with a certain number of carbon atoms. Such a group allows the polymer to have good wettability and adhesion to weakly polar materials; the third repeating structural unit has a soft side chain with an appropriate carbon chain length, which can increase the free volume of the polymer and give the polymer good flexibility. The pole piece containing the polymer has suitable mechanical strength and good flexibility.

[0035] In any embodiment of the present application, the initiator includes one or more of benzoyl peroxide, ammonium persulfate, potassium persulfate, and sodium thiosulfate. The above initiator can promote the addition reaction of the above monomers and promote the formation of polymers.

[0036] In a third aspect, the present application provides a binder, including the polymer of the first aspect or the polymer obtained by the method of the second aspect. The above polymer is used as a binder, and at least has the advantages of the polymer.

[0037] In a fourth aspect, an embodiment of the present application provides a positive electrode sheet, comprising: a positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer comprises the polymer of the first aspect or the polymer obtained by the method of the second aspect or the binder of the third aspect. The positive electrode sheet comprising the polymer or the binder has suitable mechanical strength and excellent flexibility.

[0038] In any embodiment of the present application, based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes 0.7% to 6% of a polymer or 0.7% to 6% of a binder, which may be 1% to 2.5%; or 1% to 2.5% of a polymer or a binder. When the positive electrode active material layer has the above-mentioned polymer or binder, the flexibility of the positive electrode active material layer can be improved on the basis of ensuring the mechanical strength of the positive electrode active material layer, and the probability of fracture or cracking of the positive electrode active material layer when winding or folding can be reduced.

[0039] In any embodiment of the present application, the positive electrode active material layer further comprises a positive electrode active material and a conductive agent. The positive electrode active material layer comprises a positive electrode active material and a conductive agent, and cooperates with the above-mentioned polymer to improve the mechanical strength and cohesion of the positive electrode active material layer. It can also improve the flexibility of the positive electrode sheet containing the positive electrode active material layer to avoid surface fracture or cracking during winding or folding.

[0040] In any embodiment of the present application, the average particle size Dv50 of the positive electrode active material is 1 μm to 10 μm. The average particle size Dv50 of the positive electrode active material in the above range can be better mixed with the above polymer or binder, improve the flexibility and cohesion of the positive electrode active material layer, and reduce the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer.

[0041] In any embodiment of the present application, the specific surface area of ​​the positive electrode active material is ≤15m 2 The specific surface area of ​​the positive electrode active material is within the above range, and can be more fully mixed with the above polymer or binder, thereby improving the flexibility and cohesion of the positive electrode active material layer and reducing surface fracture or cracking caused by winding or folding of the positive electrode sheet containing the positive electrode active material layer.

[0042] In any embodiment of the present application, based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes: 85%-98.7% of the positive electrode active material, optionally 91.5% to 98.3%. The content of the positive electrode active material in the positive electrode active material layer is within the above range, which can be better mixed with the above polymer or binder, improve the flexibility and cohesion of the positive electrode active material layer, and reduce the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer.

[0043] In any embodiment of the present application, based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes: 0.4% to 10% of the conductive agent, optionally 0.7% to 5%. The content of the conductive agent in the positive electrode active material layer is within the above range, which can be better mixed with the above polymer or binder, improve the flexibility and cohesive strength of the positive electrode active material layer, and reduce the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer.

[0044] In a fifth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate of the fourth aspect.

[0045] In a sixth aspect, an embodiment of the present application provides an electrical device comprising the secondary battery of the fifth aspect.

[0046] The polymer of the embodiment of the present application can be used as a binder for the positive electrode plate to improve the mechanical strength and flexibility of the positive electrode plate; the positive electrode plate, secondary battery and electrical device containing the polymer have at least the above advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some implementation methods of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0048] Figure 1 It is a schematic diagram of one embodiment of the secondary battery of the present application.

[0049] Figure 2 yes Figure 1 An exploded schematic diagram of a secondary battery is shown.

[0050] Figure 3 It is a schematic diagram of one embodiment of an electric device including the secondary battery of the present application as a power source.

[0051] In the drawings, the drawings are not necessarily drawn to scale. DETAILED DESCRIPTION

[0052] Below, the electrode assembly and its preparation method, secondary battery, battery module, battery pack and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0053] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0054] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0055] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0056] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0057] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0058] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0059] Unless otherwise specified, in this application, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0060] If not specifically stated otherwise, in this application, the term "attach" refers to connection by adhesion, coating or the like.

[0061] If not otherwise specified, in this application, the terms "first", "second", "third", "fourth", etc. are used to distinguish different objects rather than to describe a specific order or a primary and secondary relationship.

[0062] Unless otherwise specified, in this application, the term "active ions" refers to ions that can be inserted and removed between the positive and negative electrodes of a secondary battery, including but not limited to lithium ions, sodium ions, etc.

[0063] The term "multiple" as used herein refers to two or more (including two). The term "multiple" or "several" as used herein refers to two or more (including two).

[0064] "Degree of polymerization" as used in this application refers to the number of repeating units per polymer molecule or polymer segment. For example, in one or more embodiments, the degree of polymerization of the first repeating structural unit may be from about 50 to about 120, or from about 60 to about 100, or from about 70 to about 110, or from about 600 to about 90. The degree of polymerization of this application can be obtained by means commonly used in the art, such as by the detection results of MALDI-TOF, SEC-MALLS, NMR or a combination thereof of the polymer.

[0065] In the present application, the secondary battery may include a lithium-ion battery, a sodium-ion battery, etc., which is not limited in the embodiments of the present application. The secondary battery may be an aqueous battery or an oil-based battery, which is not limited in the embodiments of the present application. The secondary battery may be a flat body, a rectangular parallelepiped, or other shapes, which is not limited in the embodiments of the present application.

[0066] Secondary batteries, also known as rechargeable batteries or storage batteries, refer to batteries that can be recharged to activate active materials after being discharged and continue to be used. Generally, secondary batteries include electrode assemblies and electrolytes, and the electrode assemblies include positive electrode sheets, negative electrode sheets, and separators.

[0067] The positive electrode sheet includes a positive current collector and a positive active material layer, the positive active material layer is coated on the surface of the positive current collector, and the positive active material layer includes a positive active material and a binder. The binder is generally an organic polymer material, which is mainly used to bind the positive active material particles together to form a complete active material layer, and to bond the active material layer to the current collector surface to reduce the contact resistance as much as possible. In the preparation of the positive electrode sheet into a battery, it is necessary to go through winding, hot pressing and other processes, and in the subsequent battery charging and discharging process, the positive active material often expands and shrinks in volume. In these cases, the positive active material layer will be subjected to complex stress, and the binder needs to maintain the structural integrity of the positive active material layer and the bonding with the current collector under such complex stress. This requires the binder material to have the following properties: good cohesive strength, flexibility, and adhesion to materials of different polarities. In addition, the binder material also needs to have solubility in a given solvent such as N-methylpyrrolidone (NMP) to facilitate the preparation of a slurry for forming a positive active material layer. However, currently used binders such as polyvinylidene fluoride (PVDF), polyacrylic acid and polyacrylate binders cannot fully meet the above comprehensive performance requirements.

[0068] After research, it was found that the structure of the polymer material used as the binder can be designed so that it can meet the above-mentioned comprehensive performance requirements.

[0069] polymer

[0070] In a first aspect, an embodiment of the present application provides a polymer, comprising a first repeating structural unit shown in formula I, a second repeating structural unit shown in formula II, and a third repeating structural unit shown in formula III,

[0071]

[0072] Wherein, R1 includes an optionally substituted amide group, -R4COORc, -R6SO3R d , 3-6 membered N-containing heterocyclic group, -R7-PO(OR e )2, wherein R4 is empty or includes C1-C11 alkylene, Rc includes H, any one of optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations; R6 is empty or includes C1-C11 alkylene, R d Including H, any one of optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations; R7 is empty or includes any one of C1-C11 alkylene, -O-, and C1-C11 alkyleneoxy; R e independently include any one of H, optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations;

[0073] R2 includes any one of C4-C12 ester group, C4-C12 alkoxy acyl group, C4-C12 acyl amine group, C3-C8 cycloalkyl group, and C2-C8 heterocycloalkyl group;

[0074] R3 includes any one of C3-C12 alkyl, C3-C12 alkyl alkenyl, C4-C12 alkoxyalkyl, and substituted or unsubstituted C1-C6 acylamino;

[0075] The average polymerization degree of the first repeating structural unit is 50-120, the average polymerization degree of the second repeating structural unit is 25-60, and the average polymerization degree of the third repeating structural unit is 25-60.

[0076] In the polymer according to the embodiment of the present application, the repeating structural units with different structures give the polymer good comprehensive properties through synergistic effects, making it suitable for use as a binder in the positive electrode sheet. In the polymer, the first repeating structural unit has a group with strong polarity. On the one hand, such a group makes the polymer molecules have a strong interaction, which can improve the cohesive strength of the polymer. On the other hand, it has a strong affinity for the current collector material and the positive active material such as aluminum, so that the polymer has good wettability and adhesion to the current collector material and the positive active material; the second repeating structural unit has an ester group or alkoxy acyl group with a certain number of carbon atoms, and such a group makes the polymer have good wettability and adhesion to weak polar materials; the third repeating structural unit has a soft side chain with an appropriate carbon chain length, which can increase the free volume of the polymer and give the polymer good flexibility.

[0077] The polymer of the present application is used for the active material layer of the electrode. The polymer can provide a certain strength and flexibility for the active material layer in the positive electrode, so that the probability of the active material layer breaking and / or peeling off during the processing and use of the prepared electrode is greatly reduced.

[0078] In addition, the polymer according to the embodiment of the present application has good solubility in a solvent such as N-methylpyrrolidone (NMP), and thus has good processing performance for preparing an active material slurry and a subsequent active material layer.

[0079] In the examples of the present application, for -R4COORc, when R4 is empty, it represents a -COORc group; for -R7-PO(OR e )2, when R7 is empty, it represents -PO(OR e )2 group; for -R6SO3R d , when R6 is empty, it represents -SO3R d .

[0080] Optionally, the average degree of polymerization of the first repeating structural unit can be any value among 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120 or a range thereof. Optionally, the average degree of polymerization of the second repeating structural unit can be any value among 25, 30, 35, 40, 45, 50, 55, 60 or a range thereof. Optionally, the average degree of polymerization of the third repeating structural unit can be any value among 25, 30, 35, 40, 45, 50, 55, 60 or a range thereof. The degree of polymerization of the above structural units of the polymer within the above range can improve the adhesive properties and cohesive strength of the polymer while maintaining good flexibility. If the average degree of polymerization of the above structural units of the polymer is too low, the cohesive strength and flexibility of the polymer will be reduced; if the degree of polymerization of the above structural units of the polymer is too high, the viscosity of the polymer will increase, and the possibility of gelation will increase, and its processing performance will deteriorate.

[0081] In some optional embodiments, the polymer is a random copolymer. In the random copolymer, the first repeating structural unit, the second repeating structural unit and the third repeating structural unit are randomly distributed in the polymer chain. The random copolymer has good processing performance and bonding performance.

[0082] In some optional embodiments, the polymer comprises a block copolymer. A block copolymer is understood to be a copolymer comprising at least three block segments consisting of the above-mentioned repeating structural units with different chemical compositions. Therefore, the block copolymer of the present application may be a triblock copolymer or a multiblock copolymer. The block copolymer may be linear, branched, star-shaped, or comb-shaped, etc., and may have structures such as [A][B][C][A][C], [A][B][C], [A][B][C][A][B], [A][B][C][B], etc. Preferably, the block copolymer is a linear triblock copolymer having the structure [A][B][C]. The block copolymer may have a plurality of blocks [A], [B] and [C], in which case the block copolymer is represented, for example, as [A] x [B] y [C] z , wherein x, y and z are the degree of polymerization (DP) of the corresponding block [A], [B] or [C].

[0083] In some optional embodiments, the polymer comprises branched polymer chains. The branched polymer chains can further improve the flexibility of the above polymer and can increase the solubility of the polymer, thereby improving the processing performance of using the polymer for the preparation of the positive electrode sheet.

[0084] In some optional embodiments, the polymer comprises a linear polymer. The linear polymer can further improve the chemical stability of the polymer and reduce the possibility of degradation of the polymer chain.

[0085] In some optional embodiments, R1 comprises the structural formula: -CONH(CH2) x SO3H sulfonyl substituted amide group, -(CH2) y COOH, one or more of the 5-membered lactam rings, wherein x is an integer from 1 to 5; y is an integer from 0 to 12. Sulfonyl-substituted amide, -(CH2) y COOH and the 5-membered lactam ring have groups with strong polarity. On the one hand, such groups enable stronger interactions between polymer molecules and can improve the cohesive strength of the polymer. On the other hand, they have strong affinity for current collector materials and positive electrode active materials such as aluminum, thereby making the polymer have good wettability and adhesion to current collector materials and positive electrode active materials.

[0086] In addition, the 5-membered lactam ring in the slurry system of N-methylpyrrolidone (NMP) has a similar group to the pyrrolidone group of NMP, which can enhance the solubility of the polymer in the slurry and further improve the processing performance of the polymer.

[0087] In some optional embodiments, R1 comprises the structural formula: -CONH(CH2) x SO3H sulfonyl substituted amide group, -(CH2) y COOH, one or more of the 5-membered lactam rings, wherein x is an integer from 1 to 5; y is an integer from 0 to 12. In some optional embodiments, R1 includes -COOH, -(CH2)3COOH,

[0088] -(CH2)4COOH, -(CH2)5COOH, -(CH2)6COOH, -(CH2)7COOH, -(CH2)8COOH, -(CH2)9COOH, -(CH2) 10 COOH, -(CH2) 11 COOH, -(CH2) 12 COOH.

[0089] In some alternative embodiments, R2 comprises -COO(CH2) p CH3, where p is 2 to 10, or -OCO(CH2) qCH3, wherein q is 2 to 10. In some optional embodiments, R2 includes -COO(CH2)2CH3, -COO(CH2)3CH3, -COO(CH2)4CH3, -COO(CH2)5CH3, -COO(CH2)6CH3, -COO(CH2)7CH3, -COO(CH2)8CH3, -COO(CH2)9CH3, -COO(CH2) 10 CH3, -OCO(CH2)2CH3, -OCO(CH2)3CH3, -OCO(CH2)4CH3, -OCO(CH2)5CH3, -OCO(CH2)6CH3, -OCO(CH2)7CH3, -OCO(CH2)8CH3, -OCO(CH2)9CH3, -OCO(CH2) 10 CH3. Ester groups or alkoxy acyl groups with a certain number of carbon atoms are a type of weakly polar group that can improve the polymer's good wettability and adhesion to weakly polar materials.

[0090] In some alternative embodiments, R3 comprises -(CH2) p CH=CH2, where p is 2 to 10, or -CH2O(CH2) q CH3, wherein q is 4 to 10. In some optional embodiments, R3 includes -(CH2)2CH=CH2, -(CH2)3CH=CH2, -(CH2)4CH=CH2, -(CH2)5CH=CH2, -(CH2)6CH=CH2, -(CH2)7CH=CH2, -(CH2)8CH=CH2, -(CH2)9CH=CH2, -(CH2) 10 CH=CH2, -CH2O(CH2)4CH3, -CH2O(CH2)5CH3, -CH2O(CH2)6CH3, -CH2O(CH2)7CH3, -CH2O(CH2)8CH3, -CH2O(CH2)9CH3, -CH2O(CH2) 10 CH3.

[0091] The above-mentioned groups have soft side chains with appropriate carbon chain lengths, which can increase the free volume of the polymer and give the polymer good flexibility. When the positive electrode sheet containing the polymer is subjected to complex stresses during preparation and cycling, the sheet containing the polymer has a certain flexibility, which can reduce the probability of surface fracture or cracking of the positive electrode sheet during processing and use.

[0092] In some optional embodiments, the molar ratio of the first repeating structural unit, the second repeating structural unit and the third repeating structural unit in the polymer is 100: (20.5-120): (20.5-120). Optionally, the molar ratio of the first repeating structural unit, the second repeating structural unit and the third repeating structural unit can be 100: 20.5: 20.5, 100: 25: 20.5, 100: 30: 20.5, 100: 35: 20.5, 100: 40: 20.5, 100: 45: 20.5, 100: 50: 20.5, 100: 55: 20.5, 100: 60: 20.5, 100: 65: 20.5, 100:70:20.5, 100:75:20.5, 100:80:20.5, 100:85:20.5, 100:90:20.5, 100:95:20.5, 100:100:20.5, 100:105:20.5, 100:110:20.5, 100:115:20.5, 100:120:20.5, 100:25:25, 100:25:30, 100 :25:35, 100:25:40, 100:25:45, 100:25:50, 100:25:55, 100:25:60, 100:25:65, 100:25:70, 100:25:75, 100:25:80, 100:25:85, 100:25:90, 100:25:95, 100:25:100, 100:25:105, 100:25:110 , any ratio among 100:25:115, 100:25:120, 100:50:25, 100:60:50, 100:70:60, 100:70:70, 100:80:80, 100:90:90, 100:100:25, 100:100:100, 100:105:105, 100:110:110, 100:115:115, 100:120:120. The molar ratio of the first repeating structural unit, the second repeating structural unit and the third repeating structural unit in the polymer is within the above range, so that the cohesive strength of the polymer is within an appropriate range, and has a strong affinity for current collector materials and positive electrode active materials such as aluminum, so that the polymer has good wettability and adhesion to current collector materials and positive electrode active materials; the second repeating structural unit has an ester group or alkoxy acyl group with a certain number of carbon atoms, and such a group enables the polymer to have good wettability and adhesion to weakly polar materials; the third repeating structural unit has a soft side chain with an appropriate carbon chain length, which can increase the free volume of the polymer and give the polymer good flexibility.

[0093] In addition, in the polymer according to the present embodiment, although there is a first repeating structural unit having a strong polar functional group, the polymer also contains an appropriate amount of the second repeating structural unit and the third repeating structural unit, so that the association between the polymer and the active material (such as lithium iron phosphate) can be effectively reduced, thereby reducing the possibility of physical gelation when preparing the active material slurry. In contrast, polyacrylic acid and polyacrylate binders according to the related art contain high-density polar functional groups, which easily cause physical gelation of lithium iron phosphate slurry, thereby failing to meet the requirements of conventional wet coating.

[0094] In some optional embodiments, the molar ratio of the first repeating structural unit to the third repeating structural unit is 5:

[0095] (2~12). Optionally, the molar ratio of the first repeating structural unit to the third repeating structural unit can be any ratio of 5:2, 5:3, 5:4, 5:5, 5:6, 5:7, 5:8, 5:9, 5:10, 5:11, 5:12. When the molar ratio of the first repeating structural unit to the third repeating structural unit in the polymer is within the above range, the cohesive strength of the polymer is ensured, the similar compatibility and adhesion of the polymer to polar materials are improved, the free volume of the polymer is increased, and the polymer is given good flexibility, so that the active material layer of the electrode containing it, especially the positive active material layer of the positive electrode, has both good mechanical strength and excellent flexibility, so that the probability of the active material layer of the prepared electrode being broken and / or peeled off during processing and use is greatly reduced.

[0096] In some optional embodiments, the weight average molecular weight of the polymer is 500000-1800000, and can be 80000-1200000. The weight average molecular weight of the polymer can be any value or range composed of 500000, 600000, 700000, 800000, 900000, 1000000, 1100000, 1200000, 1300000, 1400000, 1500000, 1600000, 1700000, 1800000. When the weight average molecular weight of the polymer is within the above range, the molecular chain of the polymer has a certain length, the free volume of the polymer is increased, the change of the molecular configuration of the polymer can be increased, and the polymer is given good flexibility; the active functional groups are increased, and the bonding performance of the polymer is improved.

[0097] When the weight average molecular weight of the polymer is too small, it cannot enhance the adhesion and flexibility, and the electrode containing the polymer is relatively hard and brittle, and is easy to break during the winding process. When the weight average molecular weight of the polymer is too large, its viscosity is large, solubility is reduced, dissolution and dispersion time is increased, and manufacturing costs are increased; and its reaction activity will be greatly reduced, which will affect the viscosity and fluidity of the slurry and reduce the dynamic performance of the positive electrode containing the polymer.

[0098] The weight average molecular weight of the polymer can be measured by a method known in the art. As an example, the weight average molecular weight of the polymer in the present application can be determined by referring to the standard GB / T 21863-2008 gel permeation chromatography. Specifically, the following method can be used in the present application: using an ultra-high performance polymer chromatograph: ACQUITY APC; detector: ACQUITY differential refractive index detector. The test steps are as follows: (1) Preheating: install the chromatographic column and pipelines, turn on the console in turn, test the power supply, etc., and open the test software Empower; (2) Parameter setting, injection volume: 0μL to 50μL (depending on the sample concentration); pump flow rate: 0.2mL / min; mobile phase: 30mol / L LiBr in NMP solution; seal cleaning liquid: isopropanol; pre-column: PL gel10um MiniMIX-B Guard (size: 50mm×4.6mm×2); analytical phase: PL gel 10um MiniMIX-B (size: 250mm×4.6mm); standard: polystyrene sleeve; running time: 30min; detector: ACQUITY differential refractive index (RI) detector; column oven temperature: 90℃; detector temperature: 55℃. (3) Sample testing: a. Standard sample and test sample preparation: Weigh 0.002g to 0.004g of standard sample / test sample respectively and add 2mL of mobile phase liquid to prepare a 0.1% to 0.5% mixed standard, and place in a refrigerator for >8h; b. Standard solution / sample testing: Edit the sample group to be tested, select the established sample group method, and after the baseline is stable, click the run queue to start testing the sample; (4) Data processing: Based on the relationship between retention time and molecular weight, use the chemical workstation to establish a calibration curve, integrate and quantify the sample spectrum, and the chemical workstation automatically generates the molecular weight and molecular weight distribution results.

[0099] In some optional embodiments, the polymer has a structure shown in any one of H1-H19:

[0100]

[0101]

[0102]

[0103] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers. According to the embodiment of the present application, the electrode piece containing the compound having any of the above structures can make the electrode piece have suitable mechanical strength and better flexibility.

[0104] In a second aspect, the present application provides a method for preparing a polymer, comprising:

[0105] Mixing a monomer corresponding to the first repeating structural unit, a monomer corresponding to the second repeating structural unit, and a monomer corresponding to the third repeating structural unit with a free radical initiator in a dispersion medium to obtain a reaction mixture;

[0106] Initiate a free radical initiator to polymerize the monomer to obtain the polymer of the first aspect; wherein the monomer corresponding to the first repeating structural unit has a structural formula shown in formula Ia, R1CH=CH2(Ia), wherein R1 includes an optionally substituted amide group, -R4COORc, -R6SO3R d , 3-6 membered N-containing heterocyclic group, -R7-PO(OR e )2, wherein R4 is empty or includes C1-C11 alkylene, Rc includes H, optionally substituted ammonium ion, any one of alkali metal cation; R6 is empty or includes C1-C11 alkylene, R d Including any one of H, optionally substituted ammonium ion, and alkali metal cation; R7 is empty or includes any one of C1-C11 alkylene, -O-, and C1-C11 alkyleneoxy; R e independently comprising any one of H, optionally substituted ammonium ions, and alkali metal cations;

[0107] The monomer corresponding to the second repeating structural unit has the structural formula shown in formula II-a, R2CH=CH2(II-a),

[0108] R2 includes any one of C4-C12 ester group, C4-C12 alkoxy acyl group, C4-C12 acyl amine group, C3-C8 cycloalkyl group, and C2-C8 heterocycloalkyl group;

[0109] The monomer corresponding to the third repeating structural unit has the structural formula shown in formula III-a, R3CH=CH2(III-a),

[0110] R3 includes any one of C3-C12 alkyl, C3-C12 alkylalkenyl, C4-C12 alkoxyalkyl, and substituted or unsubstituted C1-C6 acylamino.

[0111] The preparation method of the present application has a simple process and does not require multiple complex reactions, and can be synthesized in one step. In the prepared polymer, the first repeating structural unit has a group with strong polarity. On the one hand, such a group allows a strong interaction between polymer molecules, which can improve the cohesive strength of the polymer. On the other hand, it has a strong affinity for current collector materials and positive electrode active materials such as aluminum, so that the polymer has good wettability and adhesion to current collector materials and positive electrode active materials; the second repeating structural unit has an ester group or alkoxy acyl group with a certain number of carbon atoms. Such a group allows the polymer to have good wettability and adhesion to weakly polar materials; the third repeating structural unit has a soft side chain with an appropriate carbon chain length, which can increase the free volume of the polymer and give the polymer good flexibility. The pole piece containing the polymer has suitable mechanical strength and good flexibility.

[0112] In some optional embodiments, the mass ratio of the total mass of the monomer corresponding to the first repeating structural unit, the monomer corresponding to the second repeating structural unit, and the monomer corresponding to the third repeating structural unit, the initiator, and the dispersion medium is 10: (8-15): (7-13); optionally, 10: (10-12): (9-11). By controlling the molar amounts of the above-mentioned monomers, initiators, and dispersion medium during the preparation process, on the one hand, the functionality of the obtained polymer can be increased, the weight average molecular weight of the polymer can be controlled within a suitable range, the adhesion of the polymer can be improved, and the mechanical properties and flexibility of the pole piece containing the polymer can be improved; on the other hand, the raw materials can be effectively utilized, the waste of raw materials can be avoided, and the cost can be saved.

[0113] In some optional embodiments, the end point temperature of heating is 70-110° C. Optionally, the end point temperature of heating can be any value of 70° C., 80° C., 90° C., 100° C., 110° C., or a range thereof. Controlling the end point temperature of heating within the above range can effectively allow the above monomers to undergo addition reaction; further, the reaction rate can be increased.

[0114] In some optional embodiments, the organic dispersion medium includes one or more of isopropanol, cyclohexane, and dimethyl sulfoxide. The above monomers can be in liquid form in the reaction container, and the liquid monomers can be dispersed in the organic dispersion medium, which can increase the contact opportunity between the above monomers participating in the reaction and promote the reaction.

[0115] In some optional embodiments, the initiator includes one or more of benzoyl peroxide, ammonium persulfate, potassium persulfate, and sodium thiosulfate. The above initiator can promote the addition reaction of the above monomers and promote the formation of polymers. In some embodiments, after the initiator participates in the reaction, it can be removed by recrystallization without being left behind, which is conducive to improving the purity of the polymer.

[0116] Binder

[0117] In a third aspect, the present application provides a binder, including the polymer of the first aspect or the polymer obtained by the method of the second aspect. The above polymer is used as a binder, and at least has the advantages of the polymer.

[0118] Positive electrode

[0119] In a fourth aspect, an embodiment of the present application provides a positive electrode sheet, comprising: a positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer comprises the polymer of the first aspect or the polymer obtained by the method of the second aspect or the binder of the third aspect. The positive electrode sheet comprising the polymer or the binder has suitable mechanical strength and excellent flexibility.

[0120] In some optional embodiments, based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes 0.7% to 6% of a polymer or 0.7% to 6% of a binder, optionally 1% to 2.5%; or 1% to 2.5% of a polymer or a binder. When the positive electrode active material layer has the above polymer or binder, the positive electrode active material layer has a certain cohesive strength, which can improve the flexibility of the positive electrode active material layer and reduce the probability of fracture or cracking of the positive electrode active material layer when it is wound or folded.

[0121] The positive electrode active material layer has the above-mentioned polymer or binder in the above-mentioned content. If the amount of the polymer or binder added is too low, too little binder cannot support the strength of the positive electrode active material layer, and thus cannot meet the requirements of rolling and thinning. If the amount of binder added is too large, the positive electrode active material layer will be more viscous, resulting in easy sticking of the roll during the film rolling process, and it is impossible to perform thinning and current collector composite.

[0122] In addition, since the binder itself does not have the ability to conduct ions and electrons, too much binder remaining in the pole piece will hinder the transmission of lithium ions and electrons, especially causing an increase in the interfacial charge transfer impedance; this will in turn increase the DC internal resistance of the secondary battery, reduce the charge and discharge performance including rate performance, and reduce the kinetic performance of the secondary battery. Multiple binders affect the reversible release and embedding of active ions in the positive electrode active material, affecting the cycle performance of the secondary battery. By controlling the amount of binder added to the above range, the pole piece binder content can be ensured to be moderate, and a higher proportion of positive electrode active material can be ensured. The positive pole piece has good lithium ion conductivity and electronic conductivity. Therefore, using the positive pole piece in a lithium battery can significantly improve the battery's energy density, rate performance, and cycle performance.

[0123] In some optional embodiments, the positive electrode active material layer further comprises a positive electrode active material and a conductive agent. The positive electrode active material layer comprises a positive electrode active material and a conductive agent, and cooperates with the above-mentioned polymer to improve the mechanical strength and cohesion of the positive electrode active material layer. It can also improve the flexibility of the positive electrode sheet containing the positive electrode active material layer to avoid surface fracture or cracking during winding or folding.

[0124] In some optional embodiments, the average particle size Dv50 of the positive electrode active material is 1 μm to 10 μm. The average particle size Dv50 of the positive electrode active material can be any value or a range composed of 1 μm, 2 μm, 3 μm, 3 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, and 10 μm. The average particle size Dv50 of the positive electrode active material in the above range can be better mixed with the above polymer or binder, and the positive electrode active material is more evenly dispersed, the flexibility and cohesion of the positive electrode active material layer are improved, and the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer is reduced.

[0125] In some optional embodiments, the specific surface area of ​​the positive electrode active material is ≤15 m 2 / g. The specific surface area of ​​the active material can be 1m 2 / g, 2m 2 / g, 3m 2 / g, 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, 11m 2 / g, 12m 2 / g, 13m 2 / g, 14m 2 / g, 15m 2 The specific surface area of ​​the positive electrode active material is within the above range, so that it can be more fully mixed with the above polymer or binder, thereby improving the flexibility and cohesion of the positive electrode active material layer and reducing the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer.

[0126] In some optional embodiments, based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes: 85%-98.7% of the positive electrode active material, optionally 91.5% to 98.3%. The content of the positive electrode active material in the positive electrode active material layer is within the above range, which can be better mixed with the above polymer or binder, improve the flexibility and cohesion of the positive electrode active material layer, and reduce the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer.

[0127] In some optional embodiments, based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes: 0.4% to 10% of the conductive agent, optionally 0.7% to 5%. The content of the conductive agent in the positive electrode active material layer is within the above range, which can be better mixed with the above polymer or binder, improve the flexibility and cohesion of the positive electrode active material layer, and reduce the surface fracture or cracking caused by winding or folding the positive electrode sheet containing the positive electrode active material layer.

[0128] In some embodiments, the positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector and including a positive active material. For example, the positive current collector has two surfaces opposite to each other in its thickness direction, and the positive active material layer is disposed on any one or both of the two opposite surfaces of the positive current collector.

[0129] The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material may be a positive electrode active material for a battery cell known in the art.

[0130] For example, when the battery cell is a lithium-ion battery cell or a lithium metal battery cell, the positive electrode active material may include one or more of a lithium transition metal oxide, a lithium-containing phosphate with an olivine structure, and their respective modified compounds. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium-containing phosphates with an olivine structure may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds. The present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials may also be used.

[0131] In some embodiments, in order to further improve the energy density of the battery cell, the positive electrode active material may include a general formula of Li a Ni b Co c M d O e A fOne or more of lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes one or more of N, F, S and Cl.

[0132] As an example, the positive electrode active material may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 One or more of O2, LiFePO4 and LiMnPO4.

[0133] When the secondary battery is a sodium ion battery cell or a sodium metal battery cell, the positive electrode active material may include but is not limited to one or more of sodium-containing transition metal oxides, polyanion materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.

[0134] As an example, the positive electrode active material may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, NaNi 1 / 2Ti 1 / 2 O2、NaNi 1 / 2 Mn 1 / 2 O2、Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2、NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials and general formula X p M' q (PO4) r O x Y 3-x In the general formula X p M'q (PO4) r O x Y 3-x , 0<p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2, X includes H + , Li + 、Na + , K + and NH4 + One or more of, M' is a transition metal cation, which can be selected from one or more of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion, which can be selected from one or more of F, Cl and Br.

[0135] The modified compounds of the above-mentioned positive electrode active materials may be the ones that undergo doping modification and / or surface coating modification on the positive electrode active materials.

[0136] In some embodiments, the positive electrode active material layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0137] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode binder. The present application has no particular restrictions on the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0138] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0139] The positive electrode active material layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, optional conductive agent, optional binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.

[0140] In some embodiments, the method for preparing the positive electrode active material layer includes:

[0141] Providing a slurry containing a binder, a positive electrode active material, and a conductive agent;

[0142] The slurry is coated and dried to form a positive electrode active material layer. In some embodiments, when the solid content of the slurry is ≥75%, the leveling property of the slurry disappears and the slurry can be rolled into a film by a roller press; the increase in solid content can effectively reduce drying energy consumption and reduce production costs.

[0143] In some embodiments, based on the total mass of the positive electrode active material, the conductive agent, and the binder, the total amount of the binder added is preferably 1 to 2.5 wt%, such as 1 wt%, 1.5 wt%, 2 wt%, and 2.5 wt%. If the amount of polymer or binder added is too low, too little binder cannot support the strength of the positive electrode active material layer, and thus cannot meet the requirements of rolling and thinning. If the amount of binder added is too large, the positive electrode active material layer will be more viscous, resulting in easy sticking of the roll during the membrane rolling process, and it is impossible to perform thinning and current collector composite.

[0144] Secondary battery

[0145] In a fifth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate of the fourth aspect.

[0146] The present application has no particular limitation on the type of secondary battery, for example, the secondary battery may be a lithium ion battery, a sodium ion battery, etc. A lithium ion battery may be selected.

[0147] In some embodiments, a secondary battery includes a negative electrode sheet, a separator, and an electrolyte.

[0148] [Negative electrode]

[0149] The specific composition and structure of the negative electrode plate can be selected according to the type of battery cell, and the embodiments of the present application are not limited to this.

[0150] For example, when the battery cell is a lithium-ion battery cell or a sodium-ion battery cell, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0151] The negative electrode active material is a material that can extract and embed active ions (such as lithium ions, sodium ions, etc.), and the negative electrode active material can adopt materials known in the art. As an example, the negative electrode active material includes but is not limited to one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials may also be used.

[0152] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent. As an example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0153] In some embodiments, the negative electrode film layer may further include a negative electrode binder. The present application has no particular restrictions on the type of negative electrode binder. As an example, the negative electrode binder may include styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS). One or more.

[0154] In some embodiments, the negative electrode film layer may further include other additives. As an example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC-Na), a PTC thermistor material, and the like.

[0155] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0156] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional conductive agent, optional binder, and other optional auxiliary agents in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0157] The negative electrode plate does not exclude other additional functional layers besides the negative electrode film layer. For example, in some embodiments, the negative electrode plate of the present application may also include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode plate of the present application may also include a protective layer covering the surface of the negative electrode film layer.

[0158] When the battery cell is a lithium metal battery cell, the negative electrode plate may not include negative electrode active materials capable of extracting and embedding active ions. For example, in some embodiments, the negative electrode plate may include a lithium plate or a lithium alloy plate; in other embodiments, the negative electrode plate includes a mesh or foam three-dimensional skeleton layer, such as foam copper (or copper alloy), foam nickel (or nickel alloy), copper (or copper alloy) mesh, nickel (or nickel alloy) mesh, etc.

[0159] When the battery cell is a sodium metal battery cell, the negative electrode plate may not include negative electrode active materials capable of extracting and embedding active ions. For example, in some embodiments, the negative electrode plate may include a sodium plate or a sodium alloy plate; in other embodiments, the negative electrode plate includes a mesh or foam three-dimensional skeleton layer, such as foam copper (or copper alloy), foam nickel (or nickel alloy), foam aluminum (or aluminum alloy), copper (or copper alloy) mesh, nickel (or nickel alloy) mesh, aluminum (or aluminum alloy) mesh, etc.

[0160] [Preparation method]

[0161] The preparation method of the battery of the present application is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a secondary battery cell. As an example, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the electrolyte is injected after drying. After packaging, standing, forming, shaping and other processes, a battery cell is obtained. Multiple battery cells can also be further connected in series, in parallel or in mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.

[0162] [Isolation film]

[0163] The separator is disposed between the positive electrode and the negative electrode, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting. The present application has no particular restriction on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0164] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different.

[0165] [Electrolytes]

[0166] In some embodiments, the secondary battery includes an electrolyte. The electrolyte plays a role in conducting active ions between the positive electrode plate and the negative electrode plate. The present application does not specifically limit the type of electrolyte, and it can be selected according to needs. For example, the electrolyte can include at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte).

[0167] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0168] The type of electrolyte salt is not specifically limited and can be selected according to actual needs. For example, the electrolyte salt includes one or more of lithium salts for lithium ion batteries and sodium salts for sodium ion batteries. As an example, the lithium salt includes lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalate phosphate) (LiDFOP), lithium tetrafluorooxalate phosphate (LiTFOP). As an example, the sodium salt includes one or more of NaPF6, NaClO4, NaBCl4, NaSO3CF3, and Na(CH3)C6H4SO3.

[0169] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the solvent may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE) One or more.

[0170] In some embodiments, the electrolyte may also optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature power performance.

[0171] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0172] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0173] The present application has no particular limitation on the shape of the secondary battery, which may be a flat body, a rectangular parallelepiped or other shapes. Figure 1 The secondary battery 5 is a rectangular parallelepiped structure as an example.

[0174] In some embodiments, Figure 2 As shown, the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate together form a accommodating cavity. The shell 51 has an opening connected to the accommodating cavity, and the cover plate 53 is used to cover the opening to close the accommodating cavity. The electrode assembly 52 of the first aspect of the embodiment of the present application or the electrode assembly 52 prepared by the method according to the second aspect of the embodiment of the present application is encapsulated in the accommodating cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.

[0175] The method for preparing the secondary battery of the present application is well known, and the method at least includes the step of preparing the electrode assembly of the second aspect of the embodiment of the present application. In some embodiments, the electrode assembly can be placed in an outer package, injected with electrolyte after drying, and subjected to vacuum packaging, standing, forming, shaping and other processes to obtain a secondary battery.

[0176] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.

[0177] Optionally, the battery module may further include a housing having an accommodation space, and the plurality of secondary batteries are accommodated in the accommodation space.

[0178] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0179] Electrical devices

[0180] In a sixth aspect, an embodiment of the present application provides an electrical device comprising the secondary battery of the fifth aspect.

[0181] The secondary battery or the electric device of the present application comprises the separator of the first aspect of the present application, and thus has at least the advantages of using the separator.

[0182] The secondary battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device may be, but is not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0183] Figure 3 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.

[0184] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0185] Example

[0186] The following examples describe the disclosure of the present application in more detail, and these examples are only for illustrative purposes, as it is obvious to those skilled in the art that various modifications and variations are made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0187] Example 1 Preparation of polymer H1

[0188] 298g of liquid HOOCHCH=CH2, 128g of CH2=CHCOO(CH2)3CH3 and 84g of CH2=CH(CH2)2CH2CH3 were added to the reactor in a molar ratio of 4:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, and 13g of about 0.5mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 90°C for 3h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0189]

[0190] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0191] Example 2 Preparation of polymer H2

[0192] 396g of liquid CH2=CHCONHCH2CH3, 156g of CH2=CHCOO(CH2)5CH3 and 98g of CH2=CH(CH2)3CH2CH3 were added to the reactor in a molar ratio of 4:1:1, mixed in a solvent of isopropanol under a protective atmosphere of N2, 13g of about 0.5mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 90°C for 3.5h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0193]

[0194] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0195] Example 3 Preparation of polymer H3

[0196] 644g of liquid CH2=CHCONHCH(CH3)CH2SO3H, 156g of CH2=CHCOO(CH2)5CH3 and 98g of CH2=CH(CH2)3CH2CH3 were added to the reactor in a molar ratio of 1:1:1, mixed in a solvent of isopropanol under a protective atmosphere of N2, 26g of about 1mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 95°C for 3.5h to obtain a yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0197]

[0198] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0199] Example 4 Preparation of polymer H4

[0200] 644g of liquid CH2=CHNC4H6O, 128g of CH2=CHCOO(CH2)3CH3 and 128g of CH2=CH CH2O(CH2)4CH3 were added to the reactor in a molar ratio of 4:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, and 39g of about 1.5mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 95°C for 3h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is:

[0201]

[0202] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0203] Example 5 Preparation of polymer H5

[0204] 644g of liquid CH2=CHPO3(CH2CH3)2, 86g of CH2=CHCOOCH3 and 82g of CH2=CH(CH2)2CH=CH2 were added to the reactor in a molar ratio of 4:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, and 26g of about 1.0mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 100°C for 4h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is:

[0205]

[0206] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0207] Example 6 Preparation of polymer H6

[0208] 452g of liquid CH2=CHCH2COOCH2CH3, 55g of CH2=CHCHCH3 and 86g of

[0209] CH2=CHCH2OCH2CH3 was added to the reactor in a molar ratio of 4:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, and 26g of about 1.0mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 85°C for 3.5h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0210]

[0211] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0212] Example 7 Preparation of polymer H7

[0213] 344g of liquid CH2=CHCH2COOH, 99g of CH2=CHCOOCH2CH3 and 70g of

[0214] CH2=CHCH2CH2CH3 was added to the reactor in a molar ratio of 1:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, and 26g of about 1.0mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 85°C for 3.5h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0215]

[0216] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0217] Example 8 Preparation of polymer H8

[0218] After neutralizing 340g of liquid CH2=CHCH2COOH with LiOH, 55g of CH2=CHCOOCH2CH3 and 82g of CH2=CHCH2CH2CH3 were added to the reactor in a molar ratio of 4:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, 26g of about 1.0mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 88°C for 3.5h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0219]

[0220] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0221] Example 9 Preparation of polymer H9

[0222] 344g of liquid CH2=CHCH2COOH, 97g of CH2=CHCONHCH2CH3 and 69g of

[0223] CH2=CHCH2CH2=CH2 was added to the reactor in a molar ratio of 4:1:1. Under the protective atmosphere of N2, the mixture was mixed in the solvent isopropanol. 26 g of about 1.0 mol of white powdery benzoyl peroxide was added and mixed with other substances in the reactor. The mixture was reacted at 90°C for 4 hours to obtain a light yellow solid, i.e., the polymer of this embodiment, with the structural formula

[0224]

[0225] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0226] Example 10 Preparation of polymer H10

[0227] 344 g of liquid CH2=CHCH2COOH, 110 g of CH2=CHC6H 11 With 69g

[0228] CH2=CHCH2CH2=CH2 was added to the reactor in a molar ratio of 4:1:1. Under the protective atmosphere of N2, the mixture was mixed in the solvent isopropanol. 26 g of about 1.0 mol of white powdery benzoyl peroxide was added and mixed with other substances in the reactor. The mixture was reacted at a temperature of 100°C for 5 hours to obtain a light yellow solid, i.e., the polymer of this embodiment, with the structural formula

[0229]

[0230] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0231] Example 11 Preparation of polymer H11

[0232] 440g of liquid CH2=CHCH2CONHCH2CH3, 86g of CH2=CHCH2O CH2CH3 and 69g of

[0233] CH2=CHCH2CH2=CH2 was added to the reactor in a molar ratio of 4:1:1. Under the protective atmosphere of N2, the mixture was mixed in the solvent isopropanol. 26 g of about 1.0 mol of white powdery benzoyl peroxide was added and mixed with other substances in the reactor. The mixture was reacted at a temperature of 100°C for 5 hours to obtain a light yellow solid, i.e., the polymer of this embodiment, with the structural formula

[0234]

[0235] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0236] Example 12 Preparation of polymer H12

[0237] 544g of liquid CH2=CHCH2SO3CH3, 86g of CH2=CHCH2O CH2CH3 and 69g of

[0238] CH2=CHCH2CH2=CH2 was added to the reactor in a molar ratio of 4:1:1. Under the protective atmosphere of N2, the mixture was mixed in the solvent isopropanol. 26 g of about 1.0 mol of white powdery benzoyl peroxide was added and mixed with other substances in the reactor. The mixture was reacted at a temperature of 110°C for 5 hours to obtain a light yellow solid, i.e., the polymer of this embodiment, with the structural formula

[0239]

[0240] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0241] Example 13 Preparation of polymer H13

[0242] 488g of liquid CH2=CHCH2SO3H was neutralized with NaOH, and then added to the reactor with 86g of CH2=CHCH2O CH2CH3 and 69g of CH2=CHCH2CH2=CH2 in a molar ratio of 4:1:1. The mixture was mixed in isopropanol solvent under a protective atmosphere of N2, and 26g of about 1.0mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor. The mixture was reacted at a temperature of 110°C for 5h to obtain a yellow solid, i.e., the polymer of this embodiment, with the structural formula

[0243]

[0244] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0245] Example 14 Preparation of polymer H14

[0246] 452g of liquid CH2=CHCH2CONHCH2CH3, 127g of CH2=CHCH2C4H7NH and 69g of

[0247] CH2=CHCH2CH2=CH2 was added to the reactor in a molar ratio of 4:1:1. Under the protective atmosphere of N2, the mixture was mixed in the solvent isopropanol. 26 g of about 1.0 mol of white powdery benzoyl peroxide was added and mixed with other substances in the reactor. The mixture was reacted at a temperature of 110°C for 5 hours to obtain a light yellow solid, i.e., the polymer of this embodiment, with the structural formula

[0248]

[0249] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0250] Example 15 Preparation of polymer H15

[0251] 452g of liquid CH2=CHCH2CONHCH2CH3, 127g of CH2=CHCH2C4H7NH and 100g

[0252] CH2=CHCH2OCH2CH2CH3 was added to the reactor in a molar ratio of 4:1:1, and mixed in a solvent of isopropanol under a protective atmosphere of N2, and 26g of about 1.0mol of white powdery benzoyl peroxide was added, and mixed with other substances in the reactor, and reacted at a temperature of 120°C for 5.5h to obtain a light yellow solid, i.e., the polymer of this embodiment, whose structural formula is

[0253]

[0254] Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

[0255] Comparative Example 1

[0256] The positive electrode active material, conductive agent, binder, etc. are prepared into a high solid content (75%) slurry by a kneader, and the solvent is NMP. Among them, the binder has the following structure. The positive electrode active material is lithium iron phosphate, and the conductive agent is carbon black. The content of the binder in the positive electrode active material film layer is 2wt%, the content of the conductive agent is 0.7wt%, and the content of the positive electrode active material is 97.3%.

[0257]

[0258] Wherein, x is 10 to 50, y is 10 to 25, z is 10 to 25, and x, y, and z are all positive integers.

[0259] The prepared high-solid content slurry is directly extruded to obtain a thick film with uniform thickness. The prepared positive thick film is rolled to thin to obtain a flexible film and compounded with the current collector to obtain a positive electrode sheet. The flexible film does not stick to the roller surface and is easily peeled off. The positive electrode sheet compounded with the current collector is placed in an oven for drying, and further cold pressed and cut to obtain a positive electrode sheet.

[0260] Preparation of negative electrode sheet: The negative electrode active material graphite, the conductive agent carbon black (Super P), the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) are fully stirred and mixed in a proper amount of solvent deionized water at a mass ratio of 95.4:1.5:2.5:0.6 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on one surface of the copper foil current collector, and after drying and cold pressing, a negative electrode sheet is obtained.

[0261] Preparation of isolation membrane: using porous PE membrane.

[0262] Preparation of electrolyte: Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 1:1 to obtain an organic solvent, and then lithium bis(fluorosulfonyl)imide (LiFSI) is dissolved in the above organic solvent to obtain an electrolyte, wherein the concentration of LiFSI is 1 mol / L.

[0263] Preparation of soft-pack batteries: stack the positive electrode sheet, separator, and negative electrode sheet in order to obtain an electrode assembly; place the electrode assembly in an outer packaging aluminum-plastic film, inject electrolyte after drying, and obtain a secondary battery through vacuum packaging, standing, formation, shaping and other processes.

[0264] Examples 17 to 32

[0265] The difference between Examples 17-32 and Comparative Example 1 is that the binder in the comparative example is replaced with the polymers of Examples 1-16 in sequence.

[0266] Comparative Example 2

[0267] The difference between Comparative Example 2 and Comparative Example 1 is that the binder in the comparative example is replaced by a polymer of the following structural formula, and the replacement is performed by equal mass:

[0268]

[0269] Wherein, x is 10 to 50, y is 10 to 25, z is 10 to 25, and x, y, and z are all positive integers.

[0270] Examples 33-35

[0271] The difference from Example 1 is that the content of the binder is different, and its content in the positive electrode active material film layer is as follows: 1wt%, 1.5wt%, and 2.5wt%.

[0272] Test Section

[0273] The positive electrode sheets or secondary batteries prepared in the examples and comparative examples were subjected to the following tests, and the specific test methods are as follows.

[0274] (1) Lithium deposition test

[0275] 1C constant current charge to 3.65V, then constant voltage charge to 0.05C at 3.65V, let stand for 5min, then discharge to 2.5V at 1C constant current, the above is a charge and discharge cycle of the battery, after 10 cycles, constant voltage charge to 0.05C at 3.65V. Disassemble the battery in a dry environment, the golden surface of the negative electrode indicates no decomposition, and the appearance of a silvery white area indicates decomposition.

[0276] (2) Battery cell DC internal resistance DCR performance test

[0277] Test method: At 25°C, charge at 0.33C to full charge, then discharge at 0.33C for 0.5Cn (Cn represents battery capacity) to adjust the secondary battery to 50% SOC, let stand for 30 minutes, end stand voltage V1, then discharge at 3C for 30 seconds, discharge end voltage V2, then discharge at 3C for 30 seconds, let stand for 40 seconds, charge at 3C for 30 seconds;

[0278] Calculation method: DCR = (V1-V2) / I, where V1 is the static end voltage, V2 is the discharge cut-off voltage, and I is the discharge current. The test results are shown in Table 1.

[0279] (3) Discharge rate performance test

[0280] 0.33C charge to 3.65V, constant voltage charge to current of 0.05C, stand for 5 minutes, 0.33C discharge to 2.5V and measure the discharge capacity during this period, stand for 30 minutes; 0.33C charge to 3.65V, constant voltage charge to current of 0.05C, stand for 5 minutes, 3C discharge to 2.5V and measure the discharge capacity during this period, stand for 30 minutes;

[0281] (4) Pole piece adhesion test

[0282] Cut the pole piece into a strip of 400mm long and 30mm wide with a custom-made die cutter; then take a flat thin steel plate, about 200-300mm long and 40-60mm wide, and stick a strip of double-sided tape in the center of the steel plate (the length should be greater than the sample test length, and the width should be 20mm), and smooth it with force to ensure that the double-sided tape is tightly attached to the center of the steel plate. Remove the double-sided tape and attach the pole piece to the tape; then insert the steel plate with the pole piece attached to it into the lower clamp of the tensile machine and fix it vertically; insert the pole piece without adhesive tape into the upper clamp and fix it, so that the pole piece attached to the tape is 180° with the pole piece fixed by the upper clamp. After fixing the test sample, calibrate and reset, set the test width, the electrode stripping length of 50mm, the stripping speed of 100mm / min, and then start the test. After the test is completed, the load and fixture displacement data of the stripping process can be obtained, and the bonding force can be calculated. Bonding force = load / double-sided tape width. The bonding force is plotted against the displacement to obtain the peeling force curve. The bonding force corresponding to the stable part of the curve is the bonding force of the electrode.

[0283] (5) Flexibility of the positive electrode

[0284] Take winding needles with different diameters and sort them in order of diameter size, fit the positive electrode sheets prepared in each embodiment and comparative example on the winding needles with different diameters, use an objective lens to focus on the pointed part, enlarge it 100 times, and observe whether there are cracks, until one of the positive electrode sheets on two adjacent winding needles has no cracks and the other has cracks, record the diameter of the winding needle without cracks as an indicator for assessing the flexibility of the positive electrode sheet. Note: The smaller the recorded winding needle diameter, the better the flexibility. A diameter of 1-2mm is judged as better, 3-4mm is judged as suitable, and greater than or equal to 5mm is judged as poor. Poor can detect cracking on the surface of the positive electrode active material layer.

[0285] Table 1

[0286]

[0287]

[0288] From the test results in Table 1, it can be seen that the selection of a suitable binder can improve the flexibility of the pole piece, avoid the pole piece being hard and brittle and causing the pole piece to break during the winding process, and ensure that the pole piece has sufficient bonding force to avoid delamination during the cycle process. And the amount of binder added within the appropriate range can meet the pole piece process and ensure that the battery cell has good electrochemical performance.

[0289] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A polymer, It is characterized in that It comprises a first repeating structural unit shown in formula I, a second repeating structural unit shown in formula II, and a third repeating structural unit shown in formula III, Among them, R 1 including an optionally substituted amide group, -R 4 COORc, -R 6 SO 3 R d , 3-6 membered N-containing heterocyclic group, -R 7 -PO(OR e ) 2 Any one of the following, where R 4 is empty or includes C1-C11 alkylene, Rc includes any one of H, optionally substituted ammonium ion, alkali metal cation, and alkaline earth metal cation; R 6 is empty or includes C1-C11 alkylene, R d Including H, any one of optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations; R 7 is empty or includes any one of C1-C11 alkylene, -O-, and C1-C11 alkyleneoxy; R e independently include any one of H, optionally substituted ammonium ions, alkali metal cations, and alkaline earth metal cations; R 2 Including any one of C4-C12 ester group, C4-C12 alkoxy acyl group, C4-C12 acyl amine group, C3-C8 cycloalkyl group, C2-C8 heterocycloalkyl group; R 3 Including any one of C3-C12 alkyl, C3-C12 alkyl alkenyl, C4-C12 alkoxyalkyl, substituted or unsubstituted C1-C6 acylamino; The average polymerization degree of the first repeating structural unit is 50-120, the average polymerization degree of the second repeating structural unit is 25-60, and the average polymerization degree of the third repeating structural unit is 25-60.

2. The polymer according to claim 1, It is characterized in that The polymer is a random copolymer.

3. The polymer according to claim 1 or 2, It is characterized in that The polymer comprises branched polymer chains.

4. The polymer according to any one of claims 1 to 3, It is characterized in that R 1 Including structural formula: -CONH(CH 2 ) x SO 3 H's sulfonyl-substituted amide group, -(CH 2 ) y COOH, one or more of the 5-membered lactam rings, wherein x is an integer of 1 to 5; and y is an integer of 0 to 12.

5. The polymer according to any one of claims 1 to 4, It is characterized in that R 2 Including -COO(CH 2 ) p CH 3 , or -OCO(CH 2 ) q CH 3 , wherein p is an integer from 2 to 10, and q is an integer from 2 to 10.

6. The polymer according to any one of claims 1 to 5, It is characterized in that R 3 Includes-(CH 2 ) p CH=CH 2 , -CH 2 O(CH 2 ) q CH 3 、-CH 2 O(CH 2 ) q CH 3 One or more of the following; wherein p is an integer from 2 to 10, and q is an integer from 4 to 10.

7. The polymer according to any one of claims 1 to 6, It is characterized in that The molar ratio of the first repeating structural unit, the second repeating structural unit and the third repeating structural unit is 100:(20.5-120):(20.5-120).

8. The polymer according to claim 7, It is characterized in that The molar ratio of the first repeating structural unit to the third repeating structural unit is 5:(2-12).

9. The polymer according to any one of claims 1 to 8, It is characterized in that The weight average molecular weight of the polymer is 500,000-1,800,000, and can be optionally 80,000-1,200,000.

10. The polymer according to any one of claims 1 to 9, It is characterized in that The polymer has a structure shown in any one of H1-H19: Wherein, x is 50 to 120, y is 25 to 60, z is 25 to 60, and x, y, and z are all positive integers.

11. A method for preparing a polymer, It is characterized in that include: Mixing a monomer corresponding to the first repeating structural unit, a monomer corresponding to the second repeating structural unit, and a monomer corresponding to the third repeating structural unit with a free radical initiator in a dispersion medium to obtain a reaction mixture; Initiate the free radical initiator to polymerize the monomer to obtain the polymer according to any one of claims 1 to 10; wherein, The monomer corresponding to the first repeating structural unit has the structural formula shown in Formula Ia, R 1 CH=CH 2 (Ia), R 1 Including R 1 including an optionally substituted amide group, -R 4 COORc, -R 6 SO 3 R d , 3-6 membered N-containing heterocyclic group, -R 7 -PO(OR e ) 2 Any one of the following, where R 4 is empty or includes C1-C11 alkylene, Rc includes any one of H, optionally substituted ammonium ion, and alkali metal cation; R 6 is empty or includes C1-C11 alkylene, R d Including any one of H, optionally substituted ammonium ion, alkali metal cation; R 7 is empty or includes any one of C1-C11 alkylene, -O-, and C1-C11 alkyleneoxy; R e independently include any one of H, optionally substituted ammonium ion, alkali metal cation; The monomer corresponding to the second repeating structural unit has the structural formula shown in formula II-a, R 2 CH=CH 2 (II-a), R 2 Including any one of C4-C12 ester group, C4-C12 alkoxy acyl group, C4-C12 acyl amine group, C3-C8 cycloalkyl group, C2-C8 heterocycloalkyl group; The monomer corresponding to the third repeating structural unit has the structural formula shown in formula III-a, R 3 CH=CH 2 (III-a), R 3 It includes any one of C3~C12 alkyl, C3~C12 alkyl alkenyl, C4~C12 alkoxyalkyl, and substituted or unsubstituted C1~C6 acylamino.

12. The method for preparing a polymer according to claim 11, It is characterized in that The initiator includes one or more of benzoyl peroxide, ammonium persulfate, potassium persulfate, and sodium thiosulfate.

13. A binder, It is characterized in that The invention comprises a polymer according to any one of claims 1 to 10 or a polymer prepared by the method according to any one of claims 11 or 12.

14. A positive electrode sheet, It is characterized in that include: A positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer comprises the polymer described in any one of claims 1 to 10 or the polymer prepared by the method described in claim 11 or 12 or the binder described in claim 13.

15. The positive electrode sheet according to claim 15, It is characterized in that Based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes 0.7% to 6% of the polymer or 0.7% to 6% of the binder, optionally 1% to 2.5%; or 1% to 2.5% of the polymer or the binder.

16. The positive electrode sheet according to claim 14 or 15, It is characterized in that The positive electrode active material layer further includes a positive electrode active material and a conductive agent.

17. The positive electrode sheet according to claim 16, It is characterized in that The positive electrode active material layer satisfies at least one of the following conditions: The average particle size Dv50 of the positive electrode active material is 1 μm to 10 μm; The specific surface area of ​​the positive electrode active material is ≤15m 2 / g; Based on the total weight of the positive electrode active material layer, the positive electrode active material layer comprises: 85% to 98.7% of the positive electrode active material, optionally 91.5% to 98.3%; Based on the total weight of the positive electrode active material layer, the positive electrode active material layer includes: 0.4% to 10% of the conductive agent, and optionally 0.7% to 5%.

18. A secondary battery, It is characterized in that A positive electrode sheet comprising any one of claims 14-17.

19. An electrical device, It is characterized in that Includes the secondary battery as claimed in claim 18.