Preparation method of coating dispersing agent and coating dispersing agent
By introducing polyether branched chains and methacrylic branched chains into the coating, the lack of fluidity, water retention and stability of the coating is solved, and the excellent dispersion effect and stability of the coating is achieved, thereby avoiding the Flocculation and precipitation have excellent market prospects.
Patent Information
- Application Number
- CN202410988887.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-05
AI Technical Summary
Existing paint dispersants are relatively lacking in improving the overall fluidity, water retention and mechanical properties of the paint, and are prone to flocculation and precipitation, making it difficult to ensure stability.
By mixing the starch with pure water and gelatinizing it, adding initiator, catalyst and functional monomer, and adding modified monomers after stirring reaction, forming a network structure of polyether branched chain and methacrylic branched chain, improving the coating dispersive effect and stability.
It achieves excellent dispersion effect of the paint, improves fluidity, water retention and mechanical properties, avoids flocculation and precipitation, and ensures the stability and market prospects of the paint.
Abstract
Description
Technical Field
[0001] The present application relates to the field of coatings, and in particular to a method for preparing a coating dispersant and the coating dispersant. Background Art
[0002] Paint, also known as lacquer, is a chemical film material applied to the surface of the protected or decorated substrate. It can usually form a firm continuous film with the coated substrate. It is usually composed of resin, oil, water or emulsion as the main components, and pigments, fillers, corresponding functional additives and other raw materials can also be added. In application, paint not only protects the value of the coated object, but also plays a good decorative role due to its rich colors. Nowadays, with the continuous improvement of people's environmental awareness, the development of water-based paint has been strongly advocated. Solid components such as pigments and fillers in paints occupy an important part, and their dispersion stability in the water-based system determines the performance of the paint. But at the same time, it is difficult to achieve the optimal dispersion and stabilization effect only with the help of mechanical shear force, so the use of paint dispersants is more common.
[0003] Paint dispersant is a surfactant with two opposite properties, lipophilicity and hydrophilicity, in the molecule. When preparing paint, it is difficult to achieve a good dispersion effect without the addition of paint dispersant to pigments and fillers. The paint will appear paste-like or have obvious stratification. The addition of dispersant helps to disperse the pigment particles, prevent the aggregation of pigment particles, and maintain the stability of the dispersion system.
[0004] In the prior art, although the coating dispersant has an excellent dispersing effect in the coating system, it is relatively lacking in improving other properties such as the fluidity, water retention and mechanical properties of the coating as a whole, and is also prone to flocculation, precipitation and other phenomena during use. Therefore, in order to solve the above problems, the present application provides a method for preparing a coating dispersant, and the coating dispersant prepared by the method not only has an excellent dispersing effect, but also can effectively improve the fluidity, water retention and mechanical properties of the coating as a whole, and can also ensure excellent stability during use, avoiding flocculation, precipitation and other phenomena, and has excellent market prospects. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present application provides a method for preparing a coating dispersant, and the preparation method comprises the following steps: S1: Mix the starch material and pure water and stir evenly, heat to 60-80°C and keep warm for gelatinization for 1-3 hours; S2: After the gelatinization is completed, add the initiator, catalyst and neutralizer under inert gas protection, mix evenly, add the functional monomer, and heat to 85-90°C and keep warm for 0.5-1h, then add the modified monomer dropwise, stir at 100-200r / min for 8-16h, and after the reaction is completed, dry the product to constant weight.
[0006] As a preferred solution, the starch material is at least one of hydroxypropyl distarch phosphate, acetate starch, carboxymethyl starch, hydroxymethyl starch, acetylated starch, phosphate starch, and cationic starch.
[0007] As a preferred solution, the starch material is at least one of hydroxypropyl distarch phosphate, carboxymethyl starch, acetylated starch, and phosphate starch.
[0008] As a preferred solution, the starch material is a composition of hydroxypropyl distarch phosphate and carboxymethyl starch.
[0009] As a preferred solution, the mass ratio of hydroxypropyl distarch phosphate to carboxymethyl starch is (1-2):(4-5).
[0010] As a preferred solution, the mass ratio of hydroxypropyl distarch phosphate to carboxymethyl starch is 1.5:4.5.
[0011] As a preferred solution, the mass ratio of the starch material to pure water is (1-2): (12-24).
[0012] As a preferred solution, the mass ratio of the starch material to pure water is (1-2): (15-20).
[0013] As a preferred solution, the initiator is at least one of ammonium persulfate, cerium ammonium nitrate, potassium persulfate, azobisisobutyronitrile, and benzoyl peroxide.
[0014] As a preferred solution, the initiator is a combination of ammonium persulfate and benzoyl peroxide.
[0015] As a preferred solution, the mass ratio of ammonium persulfate to benzoyl peroxide is (1-2): (1-2).
[0016] As a preferred solution, the catalyst is at least one of anhydrous aluminum chloride, boron trifluoride, carboxylic acid, aryl sulfonic acid, and boron trifluoride vinyl ether.
[0017] As a preferred solution, the catalyst is a combination of carboxylic acid and boron trifluoride vinyl ether.
[0018] As a preferred solution, the mass ratio of the carboxylic acid to boron trifluoride vinyl ether is (1.5-3): (0.5-1).
[0019] As a preferred solution, the neutralizing agent is at least one of sodium hydroxide, potassium hydroxide, sodium bicarbonate, sodium methoxide, sodium ethoxide, diethanolamine, and triethanolamine.
[0020] As a preferred solution, the neutralizing agent is diethanolamine.
[0021] As a preferred solution, the mass ratio of the initiator, the catalyst and the neutralizer is (1-2): (0.1-0.5): (4-5).
[0022] As a preferred solution, the mass ratio of the initiator, the catalyst and the neutralizer is 1.2:0.4:4.4.
[0023] As a preferred solution, the added amount of the initiator is 0.5-2wt% of the starch material.
[0024] As a preferred solution, the added amount of the initiator is 1 to 1.5 wt % of the starch material.
[0025] As a preferred solution, the functional monomer is at least one of vinyl pyrrolidone, vinyl ester, methyl acrylate, ethyl acrylate, glycidyl methacrylate, and N-isopropylacrylamide.
[0026] As a preferred solution, the functional monomer is glycidyl methacrylate.
[0027] As a preferred solution, the modified monomer is allyloxy polyethylene glycol ether.
[0028] As a preferred solution, the average molecular weight of the allyloxy polyethylene glycol ether is 1000-3000.
[0029] As a preferred solution, the average molecular weight of the allyloxy polyethylene glycol ether is 2000-2500.
[0030] As a preferred solution, the mass ratio of the starch material, the functional monomer and the modified monomer is (1-2): (0.2-0.4): (0.4-0.6).
[0031] As a preferred solution, the mass ratio of the starch material, the functional monomer and the modified monomer is (1-1.2): (0.3-0.4): (0.4-0.5).
[0032] As a preferred solution, the mass ratio of the starch material, the functional monomer and the modified monomer is 1:0.3:0.45.
[0033] A polymer coating dispersant prepared in the present application can greatly increase the density of polyether branches in the side chains of starch polymer materials by introducing functional monomers and modified monomers into starch polymer materials. The good hydrophilic effect of the polyether branches can form stable water-retaining segments in the coating system, thereby greatly reducing the movement rate and mobility of water molecules, thereby obtaining excellent water-retaining effects. The dense network structure formed by the complex branches also greatly enhances the upper limit of the stress tolerance of the coating when facing external forces, ensuring that the stress tolerance of the internal system is greatly increased. On the other hand, the combined effect of the polyether branches and the methacrylic acid branches can form a stable linked entangled network in the dispersant system and the coating system. A larger number and length of branches means a higher degree of branch cross-linking, which represents a more stable network connection force, thereby maintaining excellent self-stability as a whole, and presenting a more stable state during use and storage, avoiding the occurrence of precipitation, flocculation and precipitation.
[0034] The second aspect of the present application provides a coating dispersant prepared by the above-mentioned coating dispersant preparation method.
[0035] The beneficial effects of this application are:
[0036] 1. The present application provides a method for preparing a coating dispersant. The prepared dispersant not only has excellent dispersing effect, but also can effectively improve the overall fluidity, water retention and mechanical properties of the coating. It can also ensure excellent stability during use, avoid flocculation, precipitation and other phenomena, and has excellent market prospects.
[0037] 2. A method for preparing a coating dispersant provided in the present application can significantly increase the density of polyether branches in the side chains of starch polymer materials by introducing functional monomers and modified monomers into starch polymer materials. The good hydrophilic effect of the polyether branches can form stable water-retaining segments in the coating system, thereby significantly reducing the movement rate and mobility of water molecules, thereby obtaining an excellent water-retaining effect. The dense network structure formed by the complex branches also significantly enhances the upper limit of the stress tolerance of the coating coating when facing external forces, thereby ensuring that the stress tolerance of the internal system is significantly increased.
[0038] 3. A method for preparing a coating dispersant provided in the present application, wherein the combined effect of the polyether side chains and the methacrylic acid side chains can form a stable linked entangled network in the dispersant system and the coating system. A greater number and length of branches means a higher degree of branch cross-linking, which in turn represents a more stable network connection force, thereby maintaining excellent self-stability as a whole, and presenting a more stable state during use and storage, avoiding the occurrence of precipitation, flocculation and sedimentation. DETAILED DESCRIPTION
[0039] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0040] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0041] Example 1
[0042] Example 1 The first aspect provides a method for preparing a coating dispersant, and the preparation method comprises the following steps, measured in parts by mass: S1: Mix 100 parts of starch material with 1600 parts of pure water, stir evenly, heat to 75°C and keep warm for 2 hours; S2: After the gelatinization is completed, 1.2 parts of initiator, 0.4 parts of catalyst and 4.4 parts of neutralizer are added under inert gas protection, and 30 parts of functional monomer are added after mixing evenly, and the temperature is raised to 85°C and kept warm for 1 hour, and then 45 parts of modified monomer are added dropwise, and the reaction is stirred at 150r / min for 12 hours. After the reaction is completed, the product is vacuum dried at 60°C to constant weight.
[0043] The starch material is a combination of hydroxypropyl distarch phosphate and carboxymethyl starch, with a mass ratio of 1.5:4.5. Hydroxypropyl distarch phosphate was purchased from Xi'an Lavia Biotechnology Co., Ltd., a food-grade product sold; and carboxymethyl starch was purchased from Shandong Aicai Biotechnology Co., Ltd., a food-grade product sold.
[0044] The initiator is a combination of ammonium persulfate and benzoyl peroxide in a mass ratio of 1:2.
[0045] The catalyst is a composition of carboxylic acid and boron trifluoride vinyl ether, with a mass ratio of 2:0.8.
[0046] The neutralizing agent is diethanolamine.
[0047] The functional monomer is glycidyl methacrylate; the modified monomer is allyloxy polyethylene glycol ether, and the allyloxy polyethylene glycol ether is a product with an average molecular weight of 2400 purchased from Jiangsu Haian Petrochemical.
[0048] Example 2
[0049] Example 2 The first aspect provides a method for preparing a coating dispersant, which comprises the following steps, measured in parts by mass: S1: Mix 120 parts of starch material with 1800 parts of pure water, stir evenly, heat to 75°C and keep warm for 2 hours; S2: After the gelatinization is completed, add 1.2 parts of initiator, 0.4 parts of catalyst and 4.4 parts of neutralizer under inert gas protection, mix evenly, add 40 parts of functional monomer, heat to 85°C and keep warm for 1 hour, then add 50 parts of modified monomer dropwise, stir at 150r / min for 12 hours, and after the reaction is completed, dry the product at 60°C in a vacuum oven until constant weight is obtained.
[0050] The starch material is a combination of hydroxypropyl distarch phosphate and carboxymethyl starch, with a mass ratio of 2: 4. Hydroxypropyl distarch phosphate was purchased from Xi'an Lavia Biotechnology Co., Ltd., a food-grade product sold; and carboxymethyl starch was purchased from Shandong Aicai Biotechnology Co., Ltd., a food-grade product sold.
[0051] The initiator is a combination of ammonium persulfate and benzoyl peroxide in a mass ratio of 1:2.
[0052] The catalyst is a composition of carboxylic acid and boron trifluoride vinyl ether, with a mass ratio of 2:0.8.
[0053] The neutralizing agent is diethanolamine.
[0054] The functional monomer is glycidyl methacrylate; the modified monomer is allyloxy polyethylene glycol ether, and the allyloxy polyethylene glycol ether is a product with an average molecular weight of 2000 purchased from Jiangsu Haian Petrochemical.
[0055] Comparative Example 1
[0056] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: the preparation method of the coating dispersant includes the following steps, measured in parts by mass: S1: mixing 100 parts of starch material with 1500 parts of pure water, stirring evenly, heating to 75°C and keeping warm for 2 hours; S2: after the gelatinization is completed, 1.2 parts of initiator, 0.4 parts of catalyst and 4.4 parts of neutralizer are added under inert gas protection, and after mixing evenly, 20 parts of functional monomer are added, and the temperature is raised to 85°C and kept warm for 1 hour, and then 10 parts of modified monomer are added dropwise, and the reaction is stirred at 150r / min for 10 hours. After the reaction is completed, the product is vacuum dried at 60°C to constant weight.
[0057] Comparative Example 2
[0058] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the coating dispersant comprises the following steps, measured in parts by mass: S1: mixing 60 parts of starch material with 1800 parts of pure water, stirring evenly, heating to 75°C and keeping warm for 2 hours; S2: adding 1.2 parts of initiator, 0.4 parts of catalyst and 4.4 parts of neutralizer under inert gas protection after gelatinization, adding 60 parts of functional monomer after mixing evenly, heating to 85°C and keeping warm for 1 hour, then adding 60 parts of modified monomer dropwise, stirring at 150r / min for 12 hours, and drying the product at 60°C in vacuum to constant weight after the reaction is completed.
[0059] Comparative Example 3
[0060] The specific implementation of this comparative example is basically the same as that of Example 1, except that the functional monomer is methyl acrylate and the modifying monomer is N-isopropylacrylamide.
[0061] Comparative Example 4
[0062] The specific implementation of this comparative example is basically the same as that of Example 1, except that the catalyst is a composition of carboxylic acid and boron trifluoride vinyl ether, with a mass ratio of 4:0.5.
[0063] Comparative Example 5
[0064] The specific implementation of this comparative example is basically the same as that of Example 1, except that the modified monomer is allyloxy polyethylene glycol ether, and the allyloxy polyethylene glycol ether is purchased from Jiangsu Haian Petrochemical Co., Ltd. and has an average molecular weight of 400.
[0065] Comparative Example 6
[0066] The specific implementation of this comparative example is basically the same as that of Example 1, except that the modified monomer is allyloxy polyethylene glycol ether, and the allyloxy polyethylene glycol ether is purchased from Jiangsu Haian Petrochemical and has an average molecular weight of 4000.
[0067] Performance Evaluation
[0068] Coating test: Prepare a coating, in parts by mass: 50 parts of acrylic resin 1206, 8 parts of adhesion promoter Loxanol MI 6730, 1.5 parts of Example / Comparative Example dispersant, 0.3 parts of BYK-052 defoamer, 0.2 parts of BYK-333 leveling agent, mix, control the fineness to 20 μm, spray on a stainless steel plate, control the coating thickness to 100 μm, and perform an impact strength test with reference to GB / T1732-1993. The measured values are the average of 10 tests and recorded in Table 1.
[0069] Stability test: The coating dispersants prepared in the embodiments and comparative examples were respectively subjected to stability tests, with 50 test samples for each embodiment. The coating dispersants were placed in a constant temperature and humidity chamber at a temperature of 55±3°C and a humidity of 75% and stored for 7 days. The sample groups that showed no flocculation, precipitation, or stratification were recorded as qualified, otherwise they were unqualified. The percentage of qualified sample groups was calculated and the results were recorded in Table 1.
[0070] Table 1
[0071] Example Impact strength (kg cm) Stability test (%) Example 1 52.1 92 Example 2 49.8 90 Comparative Example 1 46.6 80 Comparative Example 2 47.4 78 Comparative Example 3 48.1 82 Comparative Example 4 44.6 76 Comparative Example 5 45.9 66 Comparative Example 6 46.1 70
[0072] From the examples and comparative examples of the present application and the data results in Table 1, it can be seen that the polymer starch dispersants introduced by the specific modified monomers and functional monomers of the present application in Examples 1 and 2 are significantly stronger than Comparative Examples 1 to 6 in terms of their own stability and coating enhancement effect. The introduction of functional monomers and modified monomers into starch polymer materials in Examples 1 and 2 can greatly increase the density of polyether branches in the side chains of starch polymer materials. Through the good hydrophilic effect of the polyether branches, stable water-retaining segments can be formed in the coating system, thereby greatly reducing the movement rate and mobility of water molecules, thereby obtaining excellent water-retaining effects. The dense network structure formed by the complex branches also greatly enhances the upper limit of the stress tolerance of the coating coating when facing external forces, ensuring that the stress tolerance of the internal system is greatly increased. On the other hand, the combined effect of the polyether branches and the methacrylic acid branches can form a stable linked entangled network in the dispersant system and the coating system. More branch numbers and lengths mean a higher degree of branch cross-linking, which represents a more stable network connection force, thereby maintaining excellent self-stability as a whole.
Claims
1. A method for preparing a coating dispersant, Features: The preparation method comprises the following steps: S1: mixing starch material and pure water, stirring evenly, heating to 60-80°C and keeping warm for 1-3 hours; S2: after the gelatinization is completed, adding initiator, catalyst and neutralizer under inert gas protection, adding functional monomer after mixing evenly, heating to 85-90°C and keeping warm for 0.5-1 hour, then adding modified monomer dropwise, stirring at 100-200 r / min for 8-16 hours, and drying the product to constant weight after the reaction is completed to obtain the product; The starch material is at least one of hydroxypropyl distarch phosphate, acetate starch, carboxymethyl starch, hydroxymethyl starch, acetylated starch, phosphate starch, and cationic starch; The mass ratio of the starch material to pure water is (1-2): (12-24); The initiator is at least one of ammonium persulfate, cerium ammonium nitrate, potassium persulfate, azobisisobutyronitrile, and benzoyl peroxide; The catalyst is at least one of anhydrous aluminum chloride, boron trifluoride, carboxylic acid, aryl sulfonic acid, and boron trifluoride vinyl ether.
2. The method for preparing a coating dispersant according to claim 1, Features: The neutralizing agent is at least one of sodium hydroxide, potassium hydroxide, sodium bicarbonate, sodium methoxide, sodium ethoxide, diethanolamine, and triethanolamine.
3. The method for preparing a coating dispersant according to claim 2, Features: The starch material is at least one of hydroxypropyl distarch phosphate, carboxymethyl starch, acetylated starch and phosphate starch.
4. The method for preparing a coating dispersant according to claim 3, Features: The starch material is a composition of hydroxypropyl distarch phosphate and carboxymethyl starch; the mass ratio of the hydroxypropyl distarch phosphate to the carboxymethyl starch is (1-2):(4-5).
5. The method for preparing a coating dispersant according to claim 4, Features: The initiator is a composition of ammonium persulfate and benzoyl peroxide; the mass ratio of the ammonium persulfate to benzoyl peroxide is (1-2): (1-2).
6. The method for preparing a coating dispersant according to claim 5, Features: The catalyst is a composition of carboxylic acid and boron trifluoride vinyl ether; the mass ratio of the carboxylic acid to the boron trifluoride vinyl ether is (1.5-3): (0.5-1).
7. The method for preparing a coating dispersant according to claim 6, Features: The mass ratio of the initiator, the catalyst and the neutralizer is (1-2): (0.1-0.5): (4-5); the added amount of the initiator is 0.5-2wt% of the starch material.
8. The method for preparing a coating dispersant according to claim 7, Features: The functional monomer is at least one of vinyl pyrrolidone, vinyl ester, methyl acrylate, ethyl acrylate, glycidyl methacrylate, and N-isopropylacrylamide.
9. The method for preparing a coating dispersant according to claim 8, Features: The modified monomer is allyloxy polyethylene glycol ether; the average molecular weight of the allyloxy polyethylene glycol ether is 1000-3000; the mass ratio of the starch material, the functional monomer and the modified monomer is (1-2): (0.2-0.4): (0.4-0.6).
10. A coating dispersant prepared by the method for preparing a coating dispersant according to any one of claims 1 to 9.