PVA polarizing film coated with free radical-cation hybrid resin and preparation method of PVA polarizing film

By coating free radical-cation mixed resin on the PVA polarizing film to form an interpenetrating polymer network structure, the deformation and intensity problems of the PVA polarizing film in a humid and heat environment are solved, and the high mechanical strength and humidity resistance are improved. Simplifies the preparation process and reduces costs.

CN118895008APending Publication Date: 2024-11-05HUAQIAO UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410935893.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The PVA polarizing film is prone to deform, shrink and has low intensity in humid and hot environments. The existing epoxy resins lack water resistance and weather resistance after curing, making it difficult to effectively combine to improve its performance.

Method used

Using a coated radical-cation mixed resin, a two-component three-dimensional crosslinking network with interpenetrating polymer network structure is formed on the surface of the PVA polarizing film, and using acrylate monomers, epoxy resins and cationic photoinitiators to act in ultraviolet light. The hybrid resin coating formed by crosslinking under the lower enhances its mechanical properties.

Benefits of technology

The deformation resistance, water resistance and mechanical strength of the PVA polarizing film are improved, the preparation process is simplified, the cost is reduced, and it is suitable for industrial mass production, and the light transmittance and moisture and heat resistance are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895008A_ABST
    Figure CN118895008A_ABST
Patent Text Reader

Abstract

The invention discloses a PVA polarizing film coated with free radical-cation hybrid resin and a preparation method. The film structurally comprises a PVA polarizing film and a free radical-cation hybrid resin coating attached to the surface of the PVA polarizing film. The free radical-cation mixed resin coating is formed by coating the surface of the PVA polarizing film with slurry and then curing the slurry. The preparation method comprises the following steps: stirring and mixing an acrylate monomer, an epoxy resin prepolymer and a cationic initiator according to a mass ratio of (1-20): 100: 5 to obtain a mixed solution, coating the surface of the PVA polarizing film with the mixed solution, and curing under the conditions that the power of ultraviolet light is 1000-4000 W and the illumination time is 30-90 s. The free radical-cation hybrid light-cured resin coating is used as a protecting and supporting film of the PVA polarizing film, so that the PVA polarizing film has good light transmittance, cohesiveness, flexibility and water vapor barrier property, the light transmittance of the polaroid is ensured, and meanwhile, the hydrophobic property of the polaroid can be greatly improved; the material can be widely used in the technical field of electronic display optical materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical materials, and in particular relates to a PVA polarizing film coated with a free radical-cationic hybrid resin and a preparation method thereof. Background Art

[0002] Polarizer is a key material in the electronic display industry, among which PVA polarizing film is the main structure to realize and determine the polarization function of polarizer. However, since PVA film is easy to absorb water, it will quickly deform, shrink and relax in a humid and hot environment after stretching treatment. In addition, the strength of PVA polarizing film is very low, and it is brittle and easy to break, which is not convenient for subsequent use and processing.

[0003] Epoxy resin is the most common hydrophobic material. Epoxy resin with certain mechanical strength can be used as a protective film to inhibit the deformation and shrinkage of PVA polarizing film. However, ordinary epoxy resin has poor water resistance and weather resistance after curing, and its mechanical strength is insufficient. The existing methods for obtaining improved epoxy resin with strong water resistance, good weather resistance and high mechanical strength often require cumbersome modification steps and have certain technical difficulties.

[0004] In view of this, how to modify epoxy resin, effectively combine epoxy resin with PVA polarizing film, and improve the performance of PVA polarizing film are technical problems that urgently need to be solved. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a PVA polarizing film coated with a free radical-cationic hybrid resin and a preparation method, which solves the problems in the above-mentioned background technology.

[0006] One of the technical solutions adopted by the present invention to solve its technical problems is: providing a PVA polarizing film coated with a free radical-cationic hybrid resin, comprising a PVA polarizing film and a free radical-cationic hybrid resin coating attached to the surface of the PVA polarizing film; the free radical-cationic hybrid resin coating has an interpenetrating polymer network structure, and the interpenetrating polymer network structure is a two-component three-dimensional cross-linked network structure formed by cross-linking and mutual penetration of epoxy resin cationic ring-opening polymerization and acrylate free radical addition polymerization under the action of a cationic photoinitiator and ultraviolet light.

[0007] In a preferred embodiment of the present invention, the free radical-cation hybrid resin coating is attached to the upper surface and the lower surface of the PVA polarizing film.

[0008] In a preferred embodiment of the present invention, the acrylate monomer includes one or more of TMPTMA (trimethylolpropane trimethacrylate), TMPTA (trimethylolpropane triacrylate) and TPGDA (tripropylene glycol diacrylate).

[0009] In a preferred embodiment of the present invention, the epoxy resin prepolymer includes bisphenol A epoxy resin, glycerol epoxy resin or aliphatic epoxy resin.

[0010] In a preferred embodiment of the present invention, the cationic initiator includes one or more of 6976 initiator (diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate), 6990 initiator (triarylsulfonium hexafluorophosphate) and 250 initiator (4-isobutylphenyl-4'-methylphenyliodonium hexafluorophosphate).

[0011] In a preferred embodiment of the present invention, the thickness of the free radical-cationic hybrid resin coating is 5 to 100 μm, and the thickness of the PVA polarizing film is 20 to 50 μm.

[0012] The second technical solution adopted by the present invention to solve the technical problem is: providing a method for preparing the above-mentioned PVA polarizing film coated with a free radical-cationic hybrid resin, comprising the following steps:

[0013] (1) mixing an acrylate monomer, an epoxy resin prepolymer, and a cationic initiator in a mass ratio of 1 to 20:100:5, and removing bubbles to obtain a mixed solution;

[0014] (2) coating the mixed solution on the surface of a PVA polarizing film, and performing ultraviolet light curing in an ultraviolet curing box, wherein the power of the ultraviolet light is 1000 to 4000 W and the illumination time is 30 to 90 seconds, to obtain a PVA polarizing film coated with a free radical-cationic hybrid resin.

[0015] In a preferred embodiment of the present invention, the mixed liquid is first coated on one side of the PVA polarizing film and cured by ultraviolet light, and then the mixed liquid is coated on the other side of the PVA polarizing film in the same manner and cured.

[0016] In a preferred embodiment of the present invention, the coating method includes spin coating, spray coating, scraper coating, brush coating, dip coating, roller coating or slit coating.

[0017] In a preferred embodiment of the present invention, the method of removing bubbles includes static debubbling, heating debubbling, vacuum debubbling or solder paste mixer debubbling.

[0018] Compared with the background technology, this technical solution has the following advantages:

[0019] 1. The present invention mixes acrylate, epoxy resin and photoinitiator together to form an interpenetrating polymer network (IPN) structure after photocuring. The characteristics of this two-component interpenetrating cross-linked network structure determine that it can have both good static and dynamic mechanical properties, giving the resin a tighter cross-linked structure and higher mechanical strength;

[0020] 2. The present invention applies the modified coating on the surface of the PVA polarizing film to improve its anti-deformation ability, thereby obtaining a PVA polarizing film with excellent water resistance, moisture and heat resistance and mechanical strength;

[0021] 3. The PVA polarizing film coated with free radical-cationic hybrid photocurable resin of the present invention requires a short curing time and has a simple preparation method, low cost, and is easy to realize industrial mass production;

[0022] 4. According to the test, the water vapor transmission rate of the PVA polarizing film coated with the free radical-cationic hybrid photocurable resin of the present invention is 6.05-7.03 g / (m 2 ·24h), the light transmittance is higher than 42%. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a flow chart of the preparation method of Examples 1-3;

[0024] Figure 2 The water vapor transmission rate of the PVA polarizing film of the embodiment and the comparative example;

[0025] Figure 3 is the light transmittance of the PVA polarizing film of the embodiment and the comparative example;

[0026] Figure 4 The following are the test results of the moisture and heat resistance of the PVA polarizing films of the embodiments and the comparative examples. DETAILED DESCRIPTION

[0027] In the following embodiments, the PVA polarizing film is preferably commercially available, and has a thickness of 20 to 50 μm, more preferably 25 to 40 μm. The thickness of the free radical-cation hybrid photocurable resin coating is preferably 5 to 100 μm, more preferably 10 to 60 μm.

[0028] In the preparation method, the power of the ultraviolet light is 1000-4000W, more preferably 3000-4000W; the illumination time is 30-90s, more preferably 30-60s. The debubbling method is preferably one or more of static debubbling, heating debubbling, vacuum debubbling and solder paste agitator debubbling. Before coating the mixed solution in step (2), the PVA polarizing film is pretreated, and the pretreatment is preferably: wiping the surface of the PVA polarizing film with anhydrous ethanol. The coating is preferably one or more of spin coating, spray coating, scraper coating, brush coating, dip coating, roller coating and slit coating.

[0029] The present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0030] Example 1

[0031] The present embodiment provides a PVA polarizing film coated with a free radical-cation hybrid photocurable resin, and the preparation method thereof comprises the following steps:

[0032] (1) 6002 bisphenol A epoxy resin, TMPTA (Shanghai Yinchang New Materials Co., Ltd.) and cationic photoinitiator 6979 (Shanghai Yinchang New Materials Co., Ltd.) were mixed and stirred evenly in a mass ratio of 100:10:5 to remove bubbles in the resin;

[0033] (2) Wipe the surface of a PVA polarizing film (25 μm, Xiangfuxing Technology Co., Ltd.) with anhydrous ethanol and dry it; coat the mixed resin on one side of the PVA polarizing film, irradiate it in a UV curing box for 50 seconds for UV curing, and then coat the mixed liquid on the other side of the PVA polarizing film, and perform the same photocuring steps to obtain a PVA polarizing film coated with a free radical-cation hybrid photocurable resin.

[0034] The PVA polarizing film coated with a free radical-cationic hybrid photocurable resin prepared in this embodiment includes a PVA polarizing film and a free radical-cationic hybrid resin coating attached to the upper and lower surfaces of the PVA polarizing film; the free radical-cationic hybrid resin coating uses acrylate monomers, epoxy resin prepolymers and cationic photoinitiators as raw materials. Under the irradiation of ultraviolet light, the cationic photoinitiator will generate strong protons to promote the ring-opening polymerization of the epoxy resin, and will also generate free radicals to promote the free radical addition polymerization of the acrylate. The two components are synergistically cured to form a two-component three-dimensional cross-linked network structure, that is, the free radical-cationic hybrid resin coating has an interpenetrating polymer network structure. The interpenetrating polymer network structure determines that it can have both good static and dynamic mechanical properties, giving the resin higher mechanical strength and improving its anti-deformation ability, so that the prepared polarizer has more excellent moisture and heat resistance. The thickness of the epoxy resin coating was measured by a thickness gauge to be 60 μm, and the water vapor permeability of the PVA polarizing film coated with free radical-cationic hybrid photocurable resin was measured by a water vapor permeability tester (38°C, 90% RH) to be 7.03 g / (m 2 ·24h).

[0035] Example 2

[0036] The preparation method of this embodiment comprises the following steps:

[0037] (1) 6002 bisphenol A epoxy resin, TMPTA (Shanghai Yinchang New Materials Co., Ltd.) and cationic photoinitiator 6979 (Shanghai Yinchang New Materials Co., Ltd.) were mixed and stirred at a mass ratio of 100:5:5 to remove bubbles in the resin;

[0038] (2) Wipe the surface of a PVA polarizing film (25 μm, Xiamen Xiangfuxing Technology Co., Ltd.) with anhydrous ethanol and dry it; coat the mixed resin on one side of the PVA polarizing film, irradiate it in a UV curing box for 50 seconds for UV curing, and then coat the mixed liquid on the other side of the PVA polarizing film, and perform the same photocuring steps to obtain a PVA polarizing film coated with a free radical-cation hybrid photocurable resin.

[0039] The thickness of the epoxy resin coating was measured by a thickness gauge to be 60 μm, and the water vapor permeability of the PVA polarizing film coated with free radical-cationic hybrid photocurable resin was measured by a water vapor permeability tester (38°C, 90% RH) to be 6.05 g / (m 2 ·24h).

[0040] Example 3

[0041] The preparation method of this embodiment comprises the following steps:

[0042] (1) 6002 bisphenol A epoxy resin, TMPTA (Shanghai Yinchang New Materials Co., Ltd.) and cationic photoinitiator 6979 (Shanghai Yinchang New Materials Co., Ltd.) were mixed and stirred at a mass ratio of 100:1:5 to remove bubbles in the resin;

[0043] (2) Wipe the surface of a PVA polarizing film (25 μm, Xiangfuxing Technology Co., Ltd.) with anhydrous ethanol and dry it; coat the mixed resin on one side of the PVA polarizing film, irradiate it in a UV curing box for 50 seconds for UV curing, and then coat the mixed liquid on the other side of the PVA polarizing film, and perform the same photocuring steps to obtain a PVA polarizing film coated with a free radical-cation hybrid photocurable resin.

[0044] The thickness of the epoxy resin coating was measured by a thickness gauge to be 60 μm, and the water vapor permeability of the PVA polarizing film coated with free radical-cationic hybrid photocurable resin was measured by a water vapor permeability tester (38°C, 90% RH) to be 7.13 g / (m 2 ·24h).

[0045] Comparative Example 1

[0046] The preparation method of the comparative example comprises the following steps:

[0047] (1) Commercially available iodine polarizer (25 μm, Xiamen Xiangfuxing Technology Co., Ltd.), wipe the surface with anhydrous ethanol and dry it;

[0048] (2) Epoxy resin was coated on one side of the PVA polarizing film, and UV-cured in a UV curing box for 50 seconds. Then epoxy resin was coated on the other side of the PVA polarizing film, and the same light-curing steps were performed to obtain a PVA polarizing film coated with light-cured epoxy resin. The water vapor permeability of the commercially available polarizer was measured by a water vapor permeability tester (38°C, 90% RH) to be 72.55 g / (m 2 ·24h).

[0049] The water vapor transmission rates of the polarizers of Examples 1 to 3 and Comparative Example 1 are as follows: Figure 2 As shown, the transmittance is Figure 3 As shown, the moisture and heat resistance test is as follows Figure 4 As shown, the light transmittance is tested by UV-visible spectrophotometer, and the moisture and heat resistance is tested by constant temperature and humidity chamber. Figure 2 , Figure 3 and Figure 4 It can be seen that the light transmittance of the PVA polarizing film coated with the free radical-cationic hybrid photocurable resin provided by the present invention is almost the same as that of the polarizer simply coated with epoxy resin, the water vapor permeability is lower, and the moisture and heat resistance performance is also better.

[0050] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A PVA polarizing film coated with a free radical-cationic hybrid resin, characterized in that: The invention comprises a PVA polarizing film and a free radical-cationic hybrid resin coating attached to the surface of the PVA polarizing film; the free radical-cationic hybrid resin coating has an interpenetrating polymer network structure, and the interpenetrating polymer network structure is a two-component three-dimensional cross-linked network structure formed by cross-linking and mutual penetration of epoxy resin cationic ring-opening polymerization and acrylate free radical addition polymerization under the action of a cationic photoinitiator and ultraviolet light.

2. The PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 1, characterized in that: The free radical-cation hybrid resin coating is attached to the upper surface and the lower surface of the PVA polarizing film.

3. The PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 1, characterized in that: The acrylate monomer includes TMPTMA, TMPTA or TPGDA.

4. The PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 1, characterized in that: The epoxy resin prepolymer includes bisphenol A epoxy resin, glycerol epoxy resin or aliphatic epoxy resin.

5. The PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 1, characterized in that: The cationic initiator includes 6976 initiator, 6990 initiator or 250 initiator.

6. The PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 1, characterized in that: The thickness of the free radical-cation mixed resin coating is 5 to 100 μm, and the thickness of the PVA polarizing film is 20 to 50 μm.

7. A method for preparing a PVA polarizing film coated with a free radical-cationic hybrid resin, characterized in that: The steps include: (1) mixing an acrylate monomer, an epoxy resin prepolymer, and a cationic initiator in a mass ratio of 1 to 20:100:5, and removing bubbles to obtain a mixed solution; (2) coating the mixed solution on the surface of a PVA polarizing film, and curing the film with ultraviolet light in an ultraviolet curing box, wherein the power of the ultraviolet light is 1000 to 4000 W and the illumination time is 30 to 90 seconds, thereby obtaining a PVA polarizing film coated with a free radical-cationic hybrid resin.

8. The method for preparing a PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 7, characterized in that: First, the mixed liquid is coated on one side of the PVA polarizing film and cured by ultraviolet light. Then, the mixed liquid is coated on the other side of the PVA polarizing film in the same manner and cured.

9. The method for preparing a PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 7, characterized in that: Coating methods include spin coating, spray coating, knife coating, brush coating, dip coating, roller coating or slot coating.

10. The method for preparing a PVA polarizing film coated with a free radical-cationic hybrid resin according to claim 7, characterized in that: The methods of removing bubbles include static debubbling, heating debubbling, vacuum debubbling or solder paste mixer debubbling.