Odor-free industrial water-based anticorrosive paint and preparation method thereof
By using specific formulas and processes of components such as plant rubber and nano-silicon sol, the problems of high VOC and flammable and explosive existing anticorrosion paints are solved, and the water-based anticorrosion paint with zero VOC, environmentally friendly and high anticorrosion performance have been achieved, significantly improving the The environmental protection and construction properties of the product.
Patent Information
- Application Number
- CN202410661012.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-11-05
AI Technical Summary
The existing anticorrosion paint has high VOC content, is flammable and explosive, causing harm to the human body and the environment, and has poor environmental protection performance.
Using plant rubber, nano-silicon sol, emulsifier and other components, a odor-cleaning industrial water-based anticorrosion paint is prepared through specific formulas and processes to ensure zero VOC, environmental protection and good anticorrosion performance.
It has achieved zero VOC anticorrosion paint, with excellent anticorrosion performance, environmental protection, weather resistance, decorative and construction properties, far exceeding the anticorrosion coatings produced by water-based resins and oil-based resins on the market.
Abstract
Description
Technical Field
[0001] The invention relates to anticorrosive paint, and specifically provides a clean-smell industrial water-based anticorrosive paint and a preparation method thereof. Background Art
[0002] At present, when manufacturing industrial water-based paint, oily resins and water-based alkyd resins are mainly used as adhesives, and pigments, fillers and various additives are used to produce paints with anti-corrosion functions. Although this kind of paint has a certain effect in anti-corrosion, it also has the following disadvantages: 1. No matter what resin is used to produce the anti-corrosion paint, it has an extremely high VOC content and poor environmental performance.
[0003] 2. Anti-corrosion paint produced by oily resin is flammable and explosive, and has extremely high VOC, which is extremely harmful to the human body and the environment.
[0004] 3. Although the anti-corrosion paint produced by water-based resin has changed the flammability and explosiveness of oil-based paint and reduced the VOC content, it still has a content of 80 ml / M2, which is harmful to the human body and pollutes the environment. VOC is a class of volatile organic compounds. Long-term exposure to low concentrations of VOC may have adverse effects on the human body, such as dizziness, fatigue, nausea and other symptoms. At high concentrations, VOC can even cause damage to the central nervous system, liver, kidneys and other organs. In addition, VOC may also cause air quality deterioration and aggravate indoor air pollution.
[0005] Therefore, it is necessary to develop more environmentally friendly and healthier anti-corrosion paints. Summary of the invention
[0006] In order to overcome the above defects, the present invention provides a clean odor industrial water-based anti-corrosion paint and a preparation method thereof. The anti-corrosion paint is clean odor, environmentally friendly and has good anti-corrosion effect.
[0007] In a first aspect, the present invention provides a clean industrial water-based anti-corrosion paint, comprising the following components in parts by weight: 100-200 parts of water, 0.1-0.5 parts of dispersant, 15-25 parts of vegetable rubber, 2-5 parts of emulsifier, 10-25 parts of nano silica sol, 20-35 parts of anticorrosive filler, 5-15 parts of pigment, 0.01-0.05 parts of defoamer and 0.01-0.03 parts of thickener.
[0008] Further, the following components are included in parts by weight: 150 parts of water, 0.3 parts of dispersant, 20 parts of vegetable rubber, 3 parts of emulsifier, nano silica sol 20 parts, antiseptic filler 23 parts, pigment 10 parts, defoamer 0.03 parts and thickener 0.02 parts.
[0009] Furthermore, the emulsifier is OP-10 emulsifier; and the vegetable rubber is Hevea brasiliensis.
[0010] Furthermore, the particle size of the nano-silica sol is 7-10 nm.
[0011] In a second aspect, the present invention further provides a method for preparing the anticorrosive paint as described in the first aspect, the preparation method comprising the following steps: S1, weighing water, dispersant, vegetable rubber, emulsifier, nano silica sol, anticorrosive filler, pigment, defoamer and thickener according to a preset ratio; S2, preparing a vegetable rubber emulsion, wherein the vegetable rubber emulsion comprises vegetable rubber, water and an emulsifier, and the weight ratio of the vegetable rubber to the water is 1:(0.8-1.2); S3, mixing the remaining water, the vegetable rubber emulsion prepared in step S1, the dispersant, the antiseptic filler, the pigment and the defoaming agent; S4, dispersing the mixture obtained after mixing in step S3 uniformly and then grinding; S5, mixing the mixture ground in step S4 with the nano-silica sol under stirring; S6, after mixing in step S5, the mixture obtained is stirred evenly and then a thickener is added.
[0012] Further, in step S2, the preparation of the vegetable rubber emulsion comprises: S21, mixing the vegetable rubber and water, and heating at 100° C. to 130° C. until the vegetable rubber is dissolved; S22, after adding the emulsifier, continue the reaction for 1-3 hours.
[0013] Furthermore, in step S21, the heating temperature is 120° C. and the heating time is 2 h.
[0014] Furthermore, in step S22, the reaction time is 2 hours.
[0015] Furthermore, the step S22 further includes a step S23 of cooling the temperature to 25-45° C. for standby use.
[0016] Furthermore, in the step S4, the mixture obtained after mixing in step S3 is dispersed uniformly and then ground, which comprises: Dispersing the mixture obtained after mixing in step S3 at 300-400 rpm; After uniform dispersion, grind to achieve a particle size of 30-40 microns; In the steps S5 and S6, the stirring rate is 300-400 rpm.
[0017] The above one or more technical solutions of the present invention have at least one or more of the following beneficial effects: The present invention provides a odorless industrial water-based anticorrosive paint and a preparation method thereof. The odorless industrial water-based anticorrosive paint not only has good anticorrosive performance, but also has the advantages of being odorless, environmentally friendly and achieving zero VOC. DETAILED DESCRIPTION
[0018] Some embodiments of the present invention are described below. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0019] Example 1 This embodiment provides an odorless industrial water-based anticorrosive paint, comprising the following components in parts by weight: 150 parts of water, 0.3 parts of dispersant, 20 parts of vegetable rubber, 3 parts of emulsifier, 20 parts of nano silica sol, 23 parts of anticorrosive filler, 10 parts of pigment, 0.03 parts of defoamer and 0.02 parts of thickener.
[0020] Example 2 This embodiment provides an odorless industrial water-based anticorrosive paint, comprising the following components in parts by weight: 100 parts of water, 0.5 parts of dispersant, 15 parts of vegetable rubber, 3 parts of emulsifier, 18 parts of nano silica sol, 30 parts of anticorrosive filler, 5 parts of pigment, 0.05 parts of defoamer and 0.01 parts of thickener.
[0021] Example 3 This embodiment provides an odorless industrial water-based anticorrosive paint, comprising the following components in parts by weight: 130 parts of water, 0.4 parts of dispersant, 25 parts of vegetable rubber, 5 parts of emulsifier, 10 parts of nano silica sol, 35 parts of anticorrosive filler, 8 parts of pigment, 0.01 parts of defoamer and 0.03 parts of thickener.
[0022] Example 4 This embodiment provides an odorless industrial water-based anticorrosive paint, comprising the following components in parts by weight: 200 parts of water, 0.1 parts of dispersant, 20 parts of vegetable rubber, 2 parts of emulsifier, 25 parts of nano silica sol, 20 parts of anticorrosive filler, 15 parts of pigment, 0.04 parts of defoamer and 0.02 parts of thickener.
[0023] In the prior art, resin is generally used as the base material of anti-corrosion paint with bonding properties. Since resin is an organic matter, it is inevitable to add components such as benzene and xylene during the synthesis process to emulsify the resin. Therefore, the existing anti-corrosion paint with resin as the base material will have a certain amount of VOC, which affects human health and pollutes the environment.
[0024] In the present invention, natural plant rubber is used and no VOC is released.
[0025] The present invention relates to a vegetable rubber, in particular, Hevea brasiliensis or Hevea brasiliensis. This type of rubber is preferred for its excellent adhesive properties and excellent water resistance. It does not dissolve in water, thereby ensuring its excellent anti-corrosion performance and greatly hindering the penetration of water vapor. Compared with some water-intolerant vegetable proteins, such as soy protein, Hevea brasiliensis is more superior in performance.
[0026] The emulsifier is preferably OP-10 emulsifier. Plant rubber such as Hevea rubber cannot exert its efficacy when used alone and needs to be emulsified. However, how to better emulsify Hevea rubber, which is a pure plant ingredient, is a difficult point. In order to better emulsify the plant rubber, the present invention uses OP-10 emulsifier. Only when Hevea rubber is fully emulsified can Hevea rubber exert its adhesiveness.
[0027] The particle size of the nano silica sol is preferably 7-10 nm. Nano silica sol has strong penetration power. At a particle size of 7-10 nm, nano silica sol can better penetrate into the hevea rubber. Because the texture of hevea rubber is relatively soft, the nano silica sol also plays a role in adjusting the hardness.
[0028] In addition, other additives, such as thickeners, can be hydroxyethyl carboxymethyl cellulose, or other common thickeners such as hydroxyethyl cellulose (HEC), polyacrylamide (PAM) and sodium polyacrylate (PAAS).
[0029] Anti-corrosion fillers such as mica iron oxide can be selected to improve the anti-corrosion performance of anti-corrosion paint.
[0030] Pigments available include iron oxide red and strontium chrome yellow.
[0031] The dispersant may be a common dispersant such as anionic polyacrylic acid sodium salt.
[0032] The water-based anticorrosive water paint produced by the present invention adopts Brazilian hevea rubber, inorganic silica sol, anticorrosive materials, pigments and fillers, additives and other materials, and has the advantages of no odor, environmental protection, good anticorrosive effect, water resistance, acid resistance, alkali resistance, convenient construction and strong decorative effect.
[0033] The invention also provides a method for preparing the anticorrosive paint.
[0034] The preparation method of the product of Example 1 comprises the following steps: S1. According to the proportions of Example 1, water, dispersant, vegetable rubber, emulsifier, nano-silica sol, antiseptic filler, pigment, defoamer and thickener are weighed respectively.
[0035] S2, preparing a vegetable rubber emulsion, wherein the vegetable rubber emulsion comprises vegetable rubber, water and an emulsifier, and the weight ratio of the vegetable rubber to the water is 1:1. The specific process of preparing the vegetable rubber emulsion comprises: S21, mixing the vegetable rubber and water, and heating at 120° C. until the vegetable rubber is dissolved; S22, after adding the emulsifier, the reaction is continued for 2 hours. After the hevea rubber and the emulsifier fully react, the hevea rubber is emulsified.
[0036] S23, cooling to 40°C, the whole system becomes a hydrophilic emulsion system for standby use.
[0037] S3, mixing the remaining water, the vegetable rubber emulsion prepared in step S1, the dispersant, the antiseptic filler, the pigment and the defoaming agent.
[0038] S4, the mixture obtained after mixing in step S3 is dispersed at 300-400 rpm. During dispersion, the speed should not be too fast, otherwise the emulsion will break. In this embodiment, the speed of this step is set to 350 rpm. After uniform dispersion, further grinding is performed. After grinding, the particles in the uniformly dispersed mixture reach a particle size of 30-40 microns, so that the mixture has good fineness, and the obtained product has good gloss, good feel, and excellent flatness, so step S4 is ground to obtain a specific fineness.
[0039] S5, mixing the mixture ground in step S4 with the nano-silica sol at a stirring rate of 300-400 rpm. During stirring, avoid demulsification and do not stir too fast. In this embodiment, the rotation speed of this step is set to 350 rpm. Since nano-silica sol is an inorganic component, it can increase the hardness and adhesion. The adhesion of Hevea rubber itself is poor. After adding nano-silica sol, the adhesion is improved. After the anti-corrosion paint is made in this way, it is sprayed on the steel, and the anti-corrosion paint and the steel can fit tightly to prevent water vapor from entering. In addition, the hardness of the anti-corrosion paint is adjusted by nano-silica sol to ensure that the anti-corrosion paint has good wear resistance, scratch resistance and stability.
[0040] S6, the mixture obtained after mixing in step S5 is stirred at a stirring rate of 300-400 rpm, and then a thickener is added and mixed evenly, and the viscosity is adjusted to the required viscosity with the thickener to obtain a finished product. In this embodiment, the speed of this step is set to 350 rpm.
[0041] The preparation method of the product of Example 2 comprises the following steps: S1. According to the proportions of Example 2, water, dispersant, vegetable rubber, emulsifier, nano-silica sol, antiseptic filler, pigment, defoamer and thickener are weighed respectively.
[0042] S2, preparing a vegetable rubber emulsion, wherein the vegetable rubber emulsion comprises vegetable rubber, water and an emulsifier, and the weight ratio of the vegetable rubber to the water is 1:0.8. The specific process of preparing the vegetable rubber emulsion comprises: S21, mixing the vegetable rubber and water, and heating at 130° C. until the vegetable rubber is dissolved; S22, after adding the emulsifier, the reaction was continued for 3 hours.
[0043] S23, cool down to 25℃, set aside S3, mixing the remaining water, the vegetable rubber emulsion prepared in step S1, the dispersant, the antiseptic filler, the pigment and the defoaming agent.
[0044] S4, dispersing the mixture obtained after mixing in step S3 at 300-400 rpm, in this embodiment, the speed of this step is set to 300 rpm, and grinding after uniform dispersion, after grinding, the particles in the uniformly dispersed mixture reach a particle size of 30-40 microns.
[0045] S5, mixing the mixture ground in step S4 with the nano-silica sol at a stirring rate of 300-400 rpm. In this embodiment, the rotation speed of this step is set to 400 rpm.
[0046] S6, the mixture obtained after mixing in step S5 is stirred at a stirring rate of 300-400 rpm, and then a thickener is added and mixed evenly, and the viscosity is adjusted to the required viscosity with the thickener to obtain a finished product. In this embodiment, the rotation speed of this step is set to 300 rpm.
[0047] The preparation method of the product of Example 3 comprises the following steps: S1. According to the proportions of Example 3, water, dispersant, vegetable rubber, emulsifier, nano-silica sol, antiseptic filler, pigment, defoamer and thickener are weighed respectively.
[0048] S2, preparing a vegetable rubber emulsion, wherein the vegetable rubber emulsion comprises vegetable rubber, water and an emulsifier, and the weight ratio of the vegetable rubber to the water is 1:1.2. The specific process of preparing the vegetable rubber emulsion comprises: S21, mixing the vegetable rubber and water, and heating at 100° C. until the vegetable rubber is dissolved; S22, after adding the emulsifier, the reaction was continued for 1 hour.
[0049] S23, cool down to 45℃, set aside S3, mixing the remaining water, the vegetable rubber emulsion prepared in step S1, the dispersant, the antiseptic filler, the pigment and the defoaming agent.
[0050] S4, dispersing the mixture obtained after mixing in step S3 at 300-400 rpm, grinding after uniform dispersion, and grinding the particles in the uniformly dispersed mixture to a particle size of 30-40 microns. In this embodiment, the rotation speed of this step is set to 400 rpm.
[0051] S5, mixing the mixture ground in step S4 with the nano-silica sol at a stirring rate of 300-400 rpm. In this embodiment, the rotation speed of this step is set to 300 rpm.
[0052] S6, the mixture obtained after mixing in step S5 is stirred at a stirring rate of 300-400 rpm, and then a thickener is added and mixed evenly, and the viscosity is adjusted to the required viscosity with the thickener to obtain a finished product. In this embodiment, the speed of this step is set to 400 rpm.
[0053] The present invention realizes the anti-corrosion paint having excellent anti-corrosion performance, strength, water resistance, dispersibility, environmental protection, etc. through a specific formula and process.
[0054] The products of Examples 1-4 were tested in accordance with GB / T38597-2020 "Technical Requirements for Coating Products with Low Volatile Organic Compound Content".
[0055] The results show that the VOC content of the anti-corrosion paints finally prepared in Examples 1-4 is less than 2 g / L, which is far below the standard of 200 g / L.
[0056] The VOC content of the anti-corrosion paint prepared by the present invention meets the requirements specified in GB / T38597-2020 "Technical Requirements for Coating Products with Low Volatile Organic Compound Content".
[0057] The odorless water-based anticorrosive paint (or coating) of the present invention is odorless and environmentally friendly, achieving zero VOC products, and its excellent anticorrosion performance, environmental protection, weather resistance, decorativeness, construction performance, and adhesion all exceed the anticorrosive coatings produced with water-based resins and oily resins in the current market.
[0058] It should be pointed out that although the various steps in the above embodiments are described in a specific order, those skilled in the art can understand that in order to achieve the effects of the present invention, different steps do not have to be performed in such an order, and they can be performed simultaneously (in parallel) or in other orders. These changes are within the scope of protection of the present invention.
[0059] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments, but it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A clean-taste industrial water-based anticorrosive paint, characterized in that: The composition comprises the following components in parts by weight: 100-200 parts of water, 0.1-0.5 parts of dispersant, 15-25 parts of vegetable rubber, 2-5 parts of emulsifier, 10-25 parts of nano silica sol, 20-35 parts of anticorrosive filler, 5-15 parts of pigment, 0.01-0.05 parts of defoamer and 0.01-0.03 parts of thickener.
2. The anticorrosive paint according to claim 1, characterized in that: The composition comprises the following components in parts by weight: 150 parts of water, 0.3 parts of dispersant, 20 parts of vegetable rubber, 3 parts of emulsifier, nano silica sol 20 parts, antiseptic filler 23 parts, pigment 10 parts, defoamer 0.03 parts and thickener 0.02 parts.
3. The anticorrosive paint according to claim 1, characterized in that: The emulsifier is OP-10 emulsifier; the vegetable rubber is three-leaf vegetable rubber.
4. The anticorrosive paint according to claim 1, characterized in that: The particle size of the nano silica sol is 7-10 nm.
5. A method for preparing an anticorrosive paint according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1, weighing water, dispersant, vegetable rubber, emulsifier, nano silica sol, anticorrosive filler, pigment, defoamer and thickener according to a preset ratio; S2, preparing a vegetable rubber emulsion, wherein the vegetable rubber emulsion comprises vegetable rubber, water and an emulsifier, and the weight ratio of the vegetable rubber to the water is 1:(0.8-1.2); S3, mixing the remaining water, the vegetable rubber emulsion prepared in step S1, the dispersant, the antiseptic filler, the pigment and the defoaming agent; S4, dispersing the mixture obtained after mixing in step S3 uniformly and then grinding; S5, mixing the mixture ground in step S4 with the nano-silica sol under stirring; S6, after mixing in step S5, the mixture obtained is stirred evenly and then a thickener is added.
6. The preparation method according to claim 5, characterized in that: In step S2, the preparation of the vegetable rubber emulsion comprises: S21, mixing the vegetable rubber and water, and heating at 100° C. to 130° C. until the vegetable rubber is dissolved; S22, after adding the emulsifier, continue the reaction for 1-3 hours.
7. The preparation method according to claim 6, characterized in that: In step S21, the heating temperature is 120°C and the heating time is 2 hours.
8. The preparation method according to claim 6, characterized in that: In step S22, the reaction time is 2 hours.
9. The preparation method according to claim 6, characterized in that: The step S22 also includes a step S23 of cooling the temperature to 25-45° C. for standby use.
10. The preparation method according to claim 5, characterized in that: In the step S4, the mixture obtained after mixing in step S3 is dispersed uniformly and then ground, which comprises: Dispersing the mixture obtained after mixing in step S3 at 300-400 rpm; After uniform dispersion, grind to achieve a particle size of 30-40 microns; In the steps S5 and S6, the stirring rate is 300-400 rpm.
Citation Information
Patent Citations
High adhesion coating for rubber articles
CA2067665A1
Anticorrosive hydrophilic coating containing chlorinated natural rubber, and preparation method thereof
CN108395770A
Water-based rubber paint, and preparation method thereof
CN108753049A
Anti-corrosion super-hydrophobic coating and preparing method and application thereof
CN109354963A
Chlorinated rubber anticorrosive paint and preparation method thereof
CN113881267A