Film material, manufacturing raw material and manufacturing method of colored layer of film material, and photoelectric device

By using curing agent containing group-NCO and organic pigments with group-NH- in the black packaging material of photovoltaic modules for cross-linking reaction, the problem of pigment migration after aging is solved, and the stability and reflection of photoelectric devices are improved , achieving more efficient power generation performance.

CN118895072AInactive Publication Date: 2024-11-05MING CROWN ADVANCED MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410904809.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The black packaging materials of existing photovoltaic modules are prone to migration of pigments after aging, resulting in color changes and reduced power generation efficiency, and existing improvements have failed to effectively solve this problem.

Method used

The cross-linking reaction is carried out using a curing agent containing group-NCO and an organic pigment with group-NH- to form a covalent bond connection, ensuring the stability of the coloring layer, and preparing film materials through specific manufacturing raw materials combinations and preparation methods. Including resins, curing agents, solvents and organic pigments, additives are added to improve weather resistance and reflectivity.

Benefits of technology

It effectively prevents pigments from migrating after aging, maintains the power stability of optoelectronic devices, and improves the reflectance of the backplane, reducing PID risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895072A_ABST
    Figure CN118895072A_ABST
Patent Text Reader

Abstract

The invention relates to the field of photoelectric packaging materials, and discloses a film material, a manufacturing raw material and a manufacturing method of a coloring layer of the film material, and a photoelectric device. The coloring layer of the film material is prepared from the following raw materials in parts by weight: resin, a curing agent, a solvent and an organic pigment; the curing agent contains a group-NCO, and the organic pigment contains a group-NH-. The preparation method of the membrane material comprises the following steps: uniformly mixing the components in the manufacturing raw materials, then coating the surface of the base membrane with the mixture, baking, curing and curing to obtain the membrane material with the coloring layer. The membrane material is prepared by the preparation method. The photoelectric device comprises the film material. The preparation raw materials of the coloring layer, the group-NCO of the curing agent and the group-NH-of the organic pigment are subjected to cross-linking reaction, so that the pigment is connected with a coating system of the coloring layer in a covalent bond form, and the problem of pigment migration after the coloring layer is aged can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optoelectronic packaging materials, and in particular to raw materials, methods and optoelectronic devices for manufacturing film materials and coloring layers thereof. Background Art

[0002] With the update of distributed and BIPV market demand, the demand for black packaging materials at the photovoltaic module end has increased. The current mainstream black packaging films include conventional black backsheets and high-reflective black backsheets. Conventional backsheets basically use carbon black or iron chromium black inorganic fillers, which have a large absorption of full-spectrum light and will reduce the packaging material's ability to reflect light, thereby reducing the power generation efficiency of photovoltaic modules.

[0003] The current mainstream high-reflective black backplane mainly improves the reflectivity of the black backplane through the high transmittance of organic pigments in the near-infrared band. According to the Qe response curve of photovoltaic modules, the increase in the reflectivity of the encapsulation film in the near-infrared band will effectively improve the power generation efficiency of photovoltaic modules. Among them, this type of near-infrared transmitting organic pigments includes perylene pigments, complex metal organic pigments, etc., which improve the reflectivity of the backplane through the transmittance of pigments to near-infrared band light. However, with the aging test of the encapsulation materials using this type of organic pigments at the module end, such as PCT, DH, UV, etc., migration and discoloration are prone to occur after aging, affecting the power of optoelectronic devices. The reason is that the photovoltaic modules encapsulated with EVA film contain 20-30% vinyl acetate in its molecular structure, and its ester bond has a large polarity. The molecular structure of the perylene pigments, complex metal organic pigments and other pigments used also contains a large number of polar groups such as imide bonds. Due to the intermolecular force between the imide bonds and the ester bonds in EVA, it is very easy for the organic pigment molecules to precipitate from the backboard material and migrate to the EVA film layer, resulting in color changes on the front of the photovoltaic module. At the same time, the aggregation of the migrated pigments on the surface of the battery reduces its power generation efficiency. By comparison, the photovoltaic modules made of POE film and the black backplane have a lower color change after aging. This is mainly because POE is a polyolefin material with a non-polar molecular structure unit, which can reduce the interfacial migration of the pigment and thus improve the discoloration. However, POE encapsulation cannot completely solve the problem of the migration of the black pigment in the backplane in the film after aging. Moreover, the single-glass modules encapsulated with POE film have an increased cost per kilowatt-hour compared to EVA film encapsulation, which is not conducive to the development of grid-parity photovoltaic modules.

[0004] Moreover, the single-glass components encapsulated with POE film have an increased electricity cost compared with EVA film encapsulation, which is not conducive to the development of grid-parity connection of photovoltaic components.

[0005] In order to improve the defects of current products, the main methods are to modify the surface of the pigment and add a barrier layer. For example, patent CN111732847A improves the weathering stability of the black backplane by coating the ultraviolet additive on the surface of the pigment. However, the pigment and the ultraviolet additive are not chemically bonded in the solution, and the stability and coating efficiency of the ultraviolet additive-coated pigment are not solved. It is very easy to have coating failure and low coating efficiency, and the color stability after aging cannot be met. Patent CN 115477867A coats styrene PS / acrylate AA monomers on the surface of the pigment to form a core-shell structure to achieve the purpose of locking the color of the pigment, but the weathering resistance of PS used in the solution needs to be evaluated and discussed, and the coating efficiency of the resin is unknown. At the same time, since the coated pigment needs to be ground by a sand mill or a ball mill with zirconium beads when used in the coating, the grinding process is easy to destroy the coating structure, which may cause the pigment coating to fail and fail to meet the pigment stability after aging. Similarly, the core-shell structure with SiO2 as the core and modified polymer resin as the outer layer used in patent CN 116344647A and patent CN 115926548A improves the migration and discoloration of pigments after aging by using silicone-modified layered fillers and adjusting the filler particle size, but both have the above-mentioned coating efficiency and subsequent coating failure problems; at the same time, patent CN 115714147A improves the migration and discoloration problem by adding a barrier layer on the surface of the black coating, but the pigment exists in the coating in a uniformly dispersed state, and the barrier coating or barrier film mentioned is an organic polymer system, the molecular pores therein cannot block the migration of the pigment in the black coating, but can only delay the migration of the pigment. Therefore, the above solutions have failed to effectively solve the migration and discoloration problem of the pigment after aging.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a raw material for manufacturing a film material and a coloring layer thereof, a manufacturing method and a photoelectric device, aiming to improve at least one of the problems mentioned in the background technology.

[0008] The present invention is achieved in that:

[0009] In a first aspect, the present invention provides a raw material for manufacturing a colored layer of a film material, comprising, by weight:

[0010] 40-60 parts of resin, 1-3 parts of curing agent, 15-65 parts of solvent and 5-12 parts of organic pigment;

[0011] The curing agent contains the group -NCO and the organic pigment contains the group -NH-.

[0012] In an optional embodiment, the invention further comprises at least one of the following technical features (1) to (4):

[0013] (1) The resin is selected from at least one of fluorocarbon resin, acrylic resin, polyester resin and polycarbonate;

[0014] (2) The curing agent is selected from at least one of HDI trimer, IPDI trimer, PDI trimer and blocked isocyanate curing agent;

[0015] (3) The solvent is selected from at least one of urethane grade ethyl acetate EA, urethane grade butyl acetate BA, and urethane grade propylene glycol monomethyl ether acetate PMA;

[0016] (4) The amount of free metal cations in the organic pigment is less than 5 ppm.

[0017] In an optional embodiment, the organic pigment is a blue organic pigment, a brown organic pigment or a purple organic pigment;

[0018] Optionally, the blue organic pigment is selected from at least one of triarylmethane lake pigments, phthalocyanine pigments, azo pigments, triphenylmethane pigments and anthraquinone pigments;

[0019] Optionally, the brown organic pigment is selected from at least one of a monoazo pigment, anthraquinone carbazole pigment and anthraquinone pigment;

[0020] Optionally, the purple organic pigment is selected from at least one of quinacridone pigments, triphenylmethane lake pigments, dioxazine pigments and condensed aromatic ring pigments.

[0021] In an optional embodiment, the invention further comprises at least one of the following technical features (1) to (7):

[0022] (1) The manufacturing raw material further includes 0.5 to 1.5 parts of a dispersant, and the dispersant is selected from at least one of BYK110 and BYK2152;

[0023] (2) The manufacturing raw materials further include 0.1 to 0.8 parts of a leveling agent, wherein the leveling agent is selected from at least one of BYK358N and BYK306;

[0024] (3) The manufacturing raw materials further include 0.6 to 2.5 parts of an ultraviolet additive, wherein the ultraviolet additive is selected from at least one of UV-400 and UV-292;

[0025] (4) The manufacturing raw materials also include 0.05 to 0.5 parts of a catalyst, and the catalyst is selected from T-12;

[0026] (5) The manufacturing raw materials further include 0.1 to 3 parts of a co-reactant, wherein the co-reactant is selected from at least one of a hydrogenated epoxy resin and an epoxy-modified polyester resin;

[0027] (6) The manufacturing raw material further includes 0.5 to 3 parts of auxiliary filler, and the auxiliary filler includes at least one of SiO2, TiO2 and ZnO. When the auxiliary filler includes TiO2, the added amount of TiO2 accounts for less than 1% by weight of the total amount of the manufacturing raw material;

[0028] (7) The acid value of the resin is ≤5.0 mg KOH / g.

[0029] In a second aspect, the present invention provides a method for preparing a membrane material, comprising:

[0030] Mixing the components of the raw materials in any of the above embodiments to obtain a coloring layer slurry;

[0031] The coloring layer slurry is coated on the surface of the base film, and then baked and cured to obtain an intermediate film material;

[0032] The intermediate film material is placed in an environment of 45-55° C. and 45-55% humidity for aging for ≥24 hours to obtain a film material with a colored layer.

[0033] In an optional embodiment, the invention further comprises at least one of the following technical features (1) to (3):

[0034] (1) The baking and curing temperature is 120 to 200° C., and the baking and curing time is 1 to 5 minutes;

[0035] (2) The method of uniformly mixing the components in the manufacturing raw materials includes:

[0036] Dividing the manufacturing raw material into a first part and a second part, wherein the first part includes the curing agent and a part of the solvent, and the second part is the substances in the manufacturing raw material except the first part;

[0037] The second part is stirred and mixed, and then ground until the particle size is ≤5 μm to obtain an intermediate slurry;

[0038] Adding the first part to the intermediate slurry and stirring evenly to obtain the coloring layer slurry;

[0039] (3) The coating thickness of the coloring layer slurry is 4 to 15 μm.

[0040] In an alternative embodiment, the reflectivity of the base film is ≥ 70%.

[0041] In an optional embodiment, the base film is a PET film, a PBT film, a modified PET film or a composite PET film;

[0042] Optionally, the material of the modified PET film is weather-resistant PET;

[0043] Optionally, the composite PET film comprises a rigid layer and a white layer, the rigid layer is a PET film, the material of the white layer is a white fluorine film or a white coating, the white layer is arranged on one side of the rigid layer, and the colored layer is arranged on the other side of the rigid layer;

[0044] The material of the white fluorine film is at least one of PVF material and PVDF material;

[0045] The material of the white coating is PU;

[0046] Optionally, the base film has a thickness of 150 to 350 μm.

[0047] In a third aspect, the present invention provides a membrane material, which is prepared by the preparation method of any one of the aforementioned embodiments;

[0048] Optionally, the surface resistivity of the black colored layer of the film material is ≥1.0×10 16 Ω.cm, and the reflectivity of the film material in the 780-1200nm band is ≥50%.

[0049] In a fourth aspect, the present invention provides a photovoltaic device, comprising the film material according to the aforementioned embodiment.

[0050] The present invention has the following beneficial effects:

[0051] The raw materials for manufacturing the coloring layer of the membrane material provided in the embodiment of the present invention are selected as components of a curing agent containing a -NCO group and an organic pigment containing a -NH- group. When the curing agent and the organic pigment are mixed, the -NCO and -NH- groups undergo a cross-linking reaction, so that the pigment and the coating system are connected in the form of a covalent bond, which can effectively improve the problem of pigment migration after aging of the coloring layer.

[0052] The method for preparing the film material provided by the present invention forms a colored layer on the surface of the base film using the manufacturing raw materials provided by the embodiment of the present invention. The pigment of the colored layer is not easy to migrate after aging, and will not affect the power of the optoelectronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0054] Figure 1 A schematic diagram of the first structure of the membrane material provided by an embodiment of the present invention;

[0055] Figure 2A schematic diagram of a second structure of a membrane material provided by an embodiment of the present invention;

[0056] Figure 3 A schematic diagram of a third structure of a membrane material provided by an embodiment of the present invention;

[0057] Figure 4 This is a statistical graph of the reflectivity of the film material prepared in Example 1 of the present invention to light of different wavelengths. DETAILED DESCRIPTION

[0058] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0059] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0060] The embodiment of the present invention provides a film material and a raw material for manufacturing a colored layer thereof, a manufacturing method and a photoelectric device.

[0061] The raw materials for manufacturing the colored layer of the film material provided in the embodiment of the present invention include, by weight:

[0062] 40-60 parts of resin, 1-3 parts of curing agent, 15-65 parts of solvent and 5-12 parts of organic pigment;

[0063] The curing agent contains the group -NCO and the organic pigment contains the group -NH-.

[0064] The raw materials for manufacturing the coloring layer of the membrane material provided in the embodiment of the present invention select a curing agent containing a -NCO group and an organic pigment containing a -NH- group as components. When the curing agent and the organic pigment are mixed, the -NCO and -NH- groups undergo a cross-linking reaction, so that the pigment and the coating system are connected in the form of a covalent bond, which can effectively improve the problem of pigment migration after aging of the coloring layer.

[0065] Preferably, the amount of free metal cations in the organic pigment used is <5 ppm.

[0066] The cause of PID in photovoltaic modules is that water vapor easily enters the edge of the module. After EVA is hydrolyzed, acetic acid is generated, which corrodes and peels off, generating a large amount of free-moving Na +, the sodium ions on the glass surface will migrate to the battery surface through the packaging material, and will react with the silver grid lines on the surface of the battery cell to corrode the battery grid lines, resulting in low filling, high series resistance, and component performance degradation. This degradation is irreversible. Conventional double-glass uses POE (polyolefin elastomer), which is a non-polar molecule with saturated bonds that are not easily hydrolyzed and has low water vapor permeability and high volume resistivity. It can largely block positively charged ions (such as Na + ) to the cell surface, reducing the PID phenomenon to a certain extent. However, in conventional single-glass modules, if free metal cations appear on the bonding surface of the backplane, the metal cations are likely to migrate to the cell surface through the back film, increasing the risk of PID. Furthermore, the residual free metal cations in the synthesis process of organic pigments may reduce the surface resistivity of the coloring layer; according to experimental data, when the surface resistivity is lower than 1.0×10 16 When Ω.cm, the PID of the component may exceed the standard.

[0067] Therefore, specifically, in terms of pigment selection, it is necessary to select pigments that have no metal cation contact during the pigment synthesis process to ensure the surface resistivity of the prepared coloring layer. Studies have found that selecting organic pigments with a free metal cation amount of less than 5ppm can effectively avoid exceeding the PID standard of the component.

[0068] Optionally, the resin is selected from at least one of fluorocarbon resin, acrylic resin, polyester resin and polycarbonate.

[0069] Optionally, the curing agent is selected from at least one of HDI trimer, IPDI trimer, PDI trimer and blocked isocyanate curing agent.

[0070] Optionally, the solvent is selected from at least one of urethane grade EA (ethyl acetate), urethane grade BA (butyl acrylate), and urethane grade PMA (propylene glycol methyl ether acetate) (dimethylaminoethyl benzoate).

[0071] Optionally, the raw material further comprises an auxiliary filler, and the auxiliary filler comprises at least one of SiO2, TiO2 and ZnO. When the auxiliary filler comprises TiO2, in order to prevent the white titanium dioxide from diluting the pigment and making the color of the coloring layer lighter, the added amount of TiO2 accounts for less than 1% by weight of the total amount of the raw material.

[0072] The addition of auxiliary fillers can improve the weather resistance of the coloring layer.

[0073] Optionally, the manufacturing raw material further includes 0.5 to 1.5 parts of a dispersant, and the dispersant is selected from at least one of BYK110 and BYK2152. The addition of the dispersant helps to make the components more evenly dispersed.

[0074] Optionally, the manufacturing raw materials further include 0.1 to 0.8 parts of a leveling agent, and the leveling agent is selected from at least one of BYK358N and BYK306. The addition of the leveling agent can promote the formation of a more flat, smooth and uniform coating film during the drying and film-forming process.

[0075] Optionally, the manufacturing raw material further includes 0.6 to 2.5 parts of an ultraviolet additive, and the ultraviolet additive is selected from at least one of UV-400 and UV-292. The addition of the ultraviolet additive helps to improve the anti-ultraviolet light irradiation ability of the coloring layer and improve the weather resistance.

[0076] Optionally, the raw materials further include 0.05 to 0.5 parts of a catalyst, wherein the catalyst is T-12. The catalyst helps to increase the curing reaction rate.

[0077] Optionally, the raw materials further include 0.1 to 3 parts of a co-reactant, which is selected from at least one of hydrogenated epoxy resin and epoxy-modified polyester resin. The addition of the co-reactant helps to increase the crosslinking reaction rate between the -NH- group of the pigment and the -NCO group of the curing agent.

[0078] Preferably, the acid value of the resin is ≤5.0 mg KOH / g. If the acid value of the resin is too high, the ring opening of the co-reactant will occur. Under the above acid value conditions, the ring opening reaction of the co-reactant can be avoided.

[0079] Optionally, the organic pigment is a blue organic pigment, a brown organic pigment or a violet organic pigment.

[0080] Furthermore, the blue organic pigment is selected from at least one of triarylmethane lake pigments, phthalocyanine pigments, azo pigments, triphenylmethane pigments and anthraquinone pigments;

[0081] Furthermore, the brown organic pigment is selected from at least one of monoazo pigments, anthraquinone carbazole pigments and anthraquinone pigments;

[0082] Furthermore, the purple organic pigment is selected from at least one of quinacridone pigments, triphenylmethane lake pigments, dioxazine pigments and condensed aromatic ring pigments.

[0083] The above pigments all contain the group -NH-, which can react with the curing agent.

[0084] The method for preparing a membrane material provided by an embodiment of the present invention comprises:

[0085] The components in the manufacturing raw materials provided in the embodiment of the present invention are mixed uniformly to obtain a coloring layer slurry;

[0086] Applying the coloring layer slurry to the surface of the base film, and baking and curing to obtain the intermediate film material;

[0087] The intermediate film material is placed at 45-55°C (e.g. 45°C, 50°C or 55°C) and 45-55% (e.g. 45%, 50% or 55%) humidity environment for ≥24h (e.g. 24, 30h, 36h or 48h, etc.) to obtain a film material with a colored layer.

[0088] The method for preparing the film material provided by the present invention can prepare a film material in which the pigment in the coloring layer is not easy to migrate by coating the coloring layer slurry made from the manufacturing raw materials provided in this embodiment on the surface of the base film.

[0089] The preparation method is specifically as follows:

[0090] S1. Pulping

[0091] The manufacturing raw materials are divided into a first part and a second part. The first part includes a curing agent and a part of a solvent; the second part is the substances in the manufacturing raw materials other than the first part, namely, resin, additives (dispersants, leveling agents, ultraviolet additives, catalysts and co-reactants), the remaining solvents, organic pigments and co-fillers.

[0092] Add the resin, additives and solvent in the second part into a mixing barrel and pre-mix thoroughly, then gradually add organic pigments and auxiliary fillers and stir to disperse evenly, stir for a certain period of time and grind until the particle size of the grinding material is ≤5μm to obtain an intermediate slurry;

[0093] The first part of the curing agent and the first part of the solvent are added to the intermediate slurry, and the mixture is stirred and diluted to form a coloring layer slurry with a solid content of 20 to 60%.

[0094] S2. Coating

[0095] The coloring layer slurry is coated on the base film using an anilox roller, the coating thickness is controlled to be 4-15 μm, and then it is placed in a drying oven at a temperature of 120-200° C. for baking and curing, and the baking and curing time is 1-5 minutes to obtain an intermediate film material.

[0096] Optionally, the base film is a PET film, a PBT film, a modified PET film or a composite PET film. PET is polyethylene terephthalate, and PBT is polybutylene terephthalate.

[0097] Optionally, the modified PET film is a weather-resistant PET film, and weather-resistant PET refers to a material in which a weather-resistant agent is added to ordinary PET for modification, wherein the weather-resistant agent may be, for example, a UV additive or the like.

[0098] Optionally, the composite PET film is a multi-layer composite film with conventional PET film as a main component.

[0099] The Qe response band of photovoltaic module cells to light is mainly concentrated in 380-1100nm, so different packaging materials of the components require different transmission or reflection capabilities in the 380-1100nm band. Photovoltaic backplanes are back packaging materials of photovoltaic modules, which can reflect the light entering the module from the front to the cells through different paths to improve the power generation efficiency of the cells. In conventional black backplanes, since carbon black and other materials have high absorption of the full spectrum band, the reflectivity of conventional black backplanes in the 380-1100nm band is generally only about 5%, and even if the reflectivity of the base film is increased, the reflectivity gain of conventional black backplanes is not obvious. When a near-infrared transmission pigment system is used to prepare a black high-reflective backplane, due to its transparent characteristics, the high transmittance of light in the coating can be guaranteed. At the same time, considering the client's requirements for the black color of the packaging material, the transmission of the coating to visible light needs to be sacrificed, so the reflectivity of the black high-reflective backplane in the visible light band will be slightly lower. However, considering the transparency of the pigment and the coating, the reflectivity of the black high-reflective backplane can also be increased when the reflectivity of the base film is increased.

[0100] Therefore, when selecting a base film, we can use a material with high reflectivity. Optionally, the reflectivity of the base film used is ≥70%.

[0101] Optionally, taking PET material as an example, weather-resistant PET or white PET is selected. For example, the reflectivity of 305 μm weather-resistant PET coated with a black coloring layer can be increased by more than 5% in the 380-1100 nm band compared to ordinary PET coated with a black coloring layer. The structure of the prepared film material is as follows: Figure 1 As shown, Figure 1 The a in the middle refers to the basement membrane.

[0102] Optionally, a composite PET film may be selected, wherein a white fluorine film or a white coating is composited on the surface of conventional PET to improve the reflectivity.

[0103] Specifically, the composite PET film includes a rigid layer and a white layer, the rigid layer is a PET film, the white layer is made of a white fluorine film or a white coating, the white layer is arranged on one side of the rigid layer, and the colored layer is arranged on the other side of the rigid layer.

[0104] The material of the white coating is PU material. The membrane structure is as follows Figure 2 As shown in the figure, a 11 Refers to white coating, a 12 Refers to the rigid layer.

[0105] The material of the white fluorine film is at least one of PVF (polyvinyl fluoride) material and PVDF (polyvinylidene fluoride) material.

[0106] Optionally, when the white layer is a white fluorine film, it is bonded to one side of the rigid layer through an adhesive layer, and the material of the adhesive layer is, for example, PU (polyurethane). Figure 3 As shown in the figure, a 21 Refers to white fluorine film, a 22 Refers to the adhesive layer, a 23 Refers to the rigid layer.

[0107] Optionally, the base film has a thickness of 150 to 350 μm (eg, 150 μm, 200 μm, 250 μm, 300 μm or 350 μm).

[0108] S3, Ripening

[0109] The intermediate film material is placed in an environment of 45-55° C. and 45-55% humidity and aged for ≥24 hours to obtain a film material with a colored layer.

[0110] The membrane material provided by the embodiment of the present invention is prepared by the preparation method provided by the embodiment of the present invention.

[0111] Optionally, the surface resistivity of the black colored layer of the film material is ≥1.0×10 16 Ω.cm, the reflectivity of the film material in the 780~1200nm band is ≥50%.

[0112] The optoelectronic device provided by the embodiment of the present invention includes the film material provided by the embodiment of the present invention.

[0113] Specifically, the film material is used as, for example, a thin film packaging material for optoelectronic devices, an insulating strip packaging material for optoelectronic devices, a reflective strip packaging material for optoelectronic devices, and the like.

[0114] A number of embodiments and comparative examples are provided below to further illustrate the present invention.

[0115] Examples 1-3 and Comparative Examples 1, 2:

[0116] Examples 1-3 and Comparative Examples 1 and 2 all provide a raw material for manufacturing a coloring layer, which includes, by weight:

[0117] 44 parts of resin, 1.2 parts of curing agent, 40 parts of solvent, 8 parts of organic pigment, 2 parts of auxiliary filler, 0.9 parts of dispersant, 0.3 parts of leveling agent, 1.5 parts of UV additive, 0.1 parts of catalyst, 2 auxiliary reactants.

[0118] Among them, the resin is a compound of acrylic resin (Tongde ACR6458) and polyester resin (Tongde AK3130), wherein the acid value of ACR6458 is 1.8 mg KOH / g, and the acid value of AK3130 is 3.9 mg KOH / g, the curing agent is Covestro N3300, the solvent is PMA (propylene glycol monomethyl ether acetate), the organic pigment is a compound (see Appendix 1 for details), the auxiliary filler is silicon dioxide and titanium dioxide, the dispersant is BYK2152, the leveling agent is BYK 358N, the ultraviolet additive is a compound of UV 400 and UV292, the catalyst is T-12, and the co-reactant is epoxy modified polyester resin (Changhao SGR-3340).

[0119] Among them, the pigment selection is different, please refer to Table 1 for details.

[0120] Examples 1 to 3 and Comparative Examples 1 and 2 all provide a method for preparing a membrane material, comprising:

[0121] Add the resin, various additives and 25 parts of solvent into the mixing barrel and pre-mix thoroughly, then gradually add the organic pigment and auxiliary filler and stir to disperse evenly, stir for a certain period of time and grind until the particle size of the grinding material is ≤5μm to obtain the intermediate slurry;

[0122] Add the curing agent and the remaining solvent to the intermediate slurry, and stir and dilute to a coloring layer slurry with a solid content of 38%;

[0123] The coloring layer slurry is coated on the base film using an anilox roller, and then placed in a drying oven at a temperature of 130° C. for baking and curing for 3 minutes to obtain an intermediate film material;

[0124] The intermediate film material is placed in a 50° C. / 50% humidity environment and aged for 24 hours to obtain a film material.

[0125] The technical details involved in the preparation process are shown in Table 2.

[0126] Table 1 Black coloring layer ingredients

[0127]

[0128]

[0129] In Table 1, pigment PV19 is purple 19 pigment (CAS: 1047-16-1), the manufacturer is SKC; pigment P.Br.28 is brown 28 pigment (CAS: 131-92-0), the manufacturer is BASF; pigment P.Br.38 is brown 38 pigment (CAS: 1126338-72-5), the manufacturer is BASF; pigment PB19 is blue 19 pigment (CAS: 58569-23-6), the manufacturer is CPMA; pigment PV55 is purple 55 pigment (CAS: 1126076-86-5), the manufacturer is DIC; pigment PB60 is blue 60 pigment (CAS: 81-77-6), the manufacturer is BASF; pigment PB (15:3) is blue 15:3 pigment (CAS: 147-14-8), the manufacturer is BASF; pigment PV23 is purple 23 pigment (CAS: 215247-95-3), the manufacturer is BSF. The pigments in the above embodiments are all pigments having a -NH- group, and the metal cation content in the pigments detected by the ICP-MS method is less than 5 ppm.

[0130] In Table 1, the pigment BASF L0086 is a 32 black pigment (CAS: 83524-75-8), manufactured by BASF; the pigment BASFX51 is an Orasol Black X 51 pigment (CAS: 12237-22-8), manufactured by BASF. All of the above pigments are pigments without the group -NH-.

[0131] Table 2 Details of membrane material preparation process

[0132]

[0133]

[0134] Embodiment 4-6

[0135] Examples 4-6 are substantially the same as Example 1, except that the component ratios are different, the specific selection of each component is different, and the operation details are different. The component ratios of Examples 4-6 are shown in Table 3, and the specific operation details are shown in Table 4:

[0136] Table 3 Group distribution ratio of Examples 4-6

[0137]

[0138]

[0139] In Table 3, pigment PV29 is purple 29 pigment (CAS: 81-33-4), manufactured by BASF; pigment P.Br.28 is brown 28 pigment (CAS: 131-92-0), manufactured by BASF; pigment P.Br.38 is brown 38 pigment (CAS: 1126338-72-5), manufactured by BASF; pigment PB60 is blue 60 pigment (CAS: 81-77-6), manufactured by BASF. The above implementation case pigments are all pigments with a -NH- group, and the metal cation content in the pigments is less than 5ppm when detected by ICP-MS method.

[0140] Table 4 Operation details of Examples 4-6

[0141] Example 4 Example 5 Example 6 Coloring layer thickness / μm 15 8 4 Base film material PET+PVDF PET+PU PET Base film thickness / μm 305 295 305 Base film (coloring layer side) color white white white

[0142] The performance of the membrane materials prepared in each embodiment and comparative example was tested. Test method:

[0143] Reflectivity test: refer to ISO 22969:2019;

[0144] Peel strength test: refer to GB / T 2790-1995;

[0145] Component preparation: 72 bifacial cells are used, and the packaging method is glass / EVA / cell / EVA / black film;

[0146] PID test: refer to IEC 62804, IEC61730-2, IEC61215.

[0147] Record the test results in Table 4-6 and Figure 4 .

[0148] Table 4 Coloring layer performance test results

[0149]

[0150]

[0151] Table 5 Test results of membrane material compression parts

[0152]

[0153] Table 6 Membrane material PID test and DH aging power attenuation

[0154]

[0155]

[0156] It can be seen from the test results in Tables 4 to 6 that the film materials prepared in the various embodiments provided by the present invention can fully meet the requirements of no migration and no discoloration during the aging process at the product application end, and the product of the present invention has a high surface resistivity, can effectively reduce the PID risk, and can provide long-term protection for optoelectronic devices.

[0157] The pigment used in Comparative Example 1 is a conventional pigment without the group -NH-, and some of the pigments used in Comparative Example 2 are conventional pigments without the group -NH-. The test results show that color migration occurs, the ΔE value (color difference) of the pressed part test result is significantly higher than that of each embodiment, and the aging power attenuation is significantly higher than that of each embodiment.

[0158] from Figure 4 It can be seen that the reflectivity of the film material prepared in Example 1 of the present invention is ≥50% in the wavelength range of 780-1200 nm.

[0159] In summary, the raw materials for manufacturing the coloring layer of the membrane material provided in the embodiment of the present invention select a curing agent containing a -NCO group and an organic pigment containing a -NH- group as components. When the curing agent and the organic pigment are mixed, the -NCO and -NH- groups undergo a cross-linking reaction, so that the pigment and the coating system are connected in the form of a covalent bond, which can effectively improve the problem of pigment migration after aging of the coloring layer.

[0160] The method for preparing the film material provided by the present invention forms a colored layer on the surface of the base film using the manufacturing raw materials provided by the embodiment of the present invention. The pigment of the colored layer is not easy to migrate after aging, and will not affect the power of the optoelectronic device.

[0161] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A raw material for manufacturing a colored layer of a film material, characterized in that: The parts by weight include: 40-60 parts of resin, 1-3 parts of curing agent, 15-65 parts of solvent and 5-12 parts of organic pigment; The curing agent contains a group -NCO, and the organic pigment contains a group -NH-.

2. The manufacturing raw material according to claim 1, characterized in that: It also includes at least one of the following technical features (1) to (4): (1) The resin is selected from at least one of fluorocarbon resin, acrylic resin, polyester resin and polycarbonate; (2) The curing agent is selected from at least one of HDI trimer, IPDI trimer, PDI trimer and blocked isocyanate curing agent; (3) The solvent is selected from at least one of urethane grade ethyl acetate EA, urethane grade butyl acetate BA, and urethane grade propylene glycol monomethyl ether acetate PMA; (4) The amount of free metal cations in the organic pigment is less than 5 ppm.

3. The manufacturing raw material according to claim 1, characterized in that The organic pigment is a blue organic pigment, a brown organic pigment or a purple organic pigment; Optionally, the blue organic pigment is selected from at least one of triarylmethane lake pigments, phthalocyanine pigments, azo pigments, triphenylmethane pigments and anthraquinone pigments; Optionally, the brown organic pigment is selected from at least one of monoazo pigments, anthraquinone carbazole pigments and anthraquinone pigments; Optionally, the purple organic pigment is selected from at least one of quinacridone pigments, triphenylmethane lake pigments, dioxazine pigments and condensed aromatic ring pigments.

4. The manufacturing raw material according to claim 1, characterized in that It also includes at least one of the following technical features (1) to (7): (1) The manufacturing raw material further includes 0.5 to 1.5 parts of a dispersant, and the dispersant is selected from at least one of BYK110 and BYK2152; (2) The manufacturing raw materials further include 0.1 to 0.8 parts of a leveling agent, wherein the leveling agent is selected from at least one of BYK358N and BYK306; (3) The manufacturing raw materials further include 0.6 to 2.5 parts of an ultraviolet additive, wherein the ultraviolet additive is selected from at least one of UV-400 and UV-292; (4) The manufacturing raw materials also include 0.05 to 0.5 parts of a catalyst, and the catalyst is selected from T-12; (5) The manufacturing raw materials further include 0.1 to 3 parts of a co-reactant, wherein the co-reactant is selected from at least one of a hydrogenated epoxy resin and an epoxy-modified polyester resin; (6) The manufacturing raw material further includes 0.5 to 3 parts of auxiliary filler, and the auxiliary filler includes at least one of SiO2, TiO2 and ZnO. When the auxiliary filler includes TiO2, the added amount of TiO2 accounts for less than 1% by weight of the total amount of the manufacturing raw material; (7) The acid value of the resin is ≤5.0 mg KOH / g.

5. A method for preparing a membrane material, characterized in that: include: Mixing the components in the manufacturing raw material according to any one of claims 1 to 4 uniformly to obtain a coloring layer slurry; The coloring layer slurry is coated on the surface of the base film, and then baked and cured to obtain an intermediate film material; The intermediate film material is placed in an environment of 45-55° C. and 45-55% humidity for aging for ≥24 hours to obtain a film material with a colored layer.

6. The preparation method according to claim 5, characterized in that: It also includes at least one of the following technical features (1) to (3): (1) The baking and curing temperature is 120 to 200° C., and the baking and curing time is 1 to 5 minutes; (2) The method of uniformly mixing the components in the manufacturing raw materials includes: Dividing the manufacturing raw material into a first part and a second part, wherein the first part includes the curing agent and a part of the solvent, and the second part is the substances in the manufacturing raw material except the first part; The second part is stirred and mixed, and then ground to a particle size of ≤5 μm to obtain an intermediate slurry; Adding the first part to the intermediate slurry and stirring evenly to obtain the coloring layer slurry; (3) The coating thickness of the coloring layer slurry is 4 to 15 μm.

7. The preparation method according to claim 5, characterized in that: The reflectivity of the base film is ≥70%.

8. The preparation method according to claim 7, characterized in that: The base film is a PET film, a PBT film, a modified PET film or a composite PET film; Optionally, the material of the modified PET film is weather-resistant PET; Optionally, the composite PET film comprises a rigid layer and a white layer, the rigid layer is a PET film, the material of the white layer is a white fluorine film or a white coating, the white layer is arranged on one side of the rigid layer, and the colored layer is arranged on the other side of the rigid layer; The material of the white fluorine film is at least one of PVF material and PVDF material; The material of the white coating is PU material; Optionally, the base film has a thickness of 150 to 350 μm.

9. A membrane material, characterized in that: Prepared by the preparation method according to any one of claims 5 to 8; Optionally, the surface resistivity of the black colored layer of the film material is ≥1.0×10 16 Ω.cm, and the reflectivity of the film material in the 780-1200nm band is ≥50%.

10. A photoelectric device, characterized in that: Comprising the membrane material as claimed in claim 9.

Citation Information

Patent Citations

  • Polyurethane resin addition pigment, process for producing polyurethane resin addition pigment, pigment dispersion composition, and jet printing ink composition

    CN103068932A

  • Pearl essence coated polymer microspheres and preparation method and application thereof

    CN104629088A

  • Colored polyurethane resin for synthetic leather and preparation method thereof

    CN104693403A

  • Packaging adhesive film for solar cell and preparation method thereof

    CN113004815A

  • Coating, solar cell backboard and assembly thereof

    CN114958064A