Light-cured jade adhesive as well as preparation method and application thereof
By using a light-cured jade adhesive, which incorporates components such as difunctional (meth)acrylate monomers, the problems of low bonding strength and environmental sensitivity of existing jade adhesives are solved, achieving a highly efficient and stable jade bonding effect.
Patent Information
- Application Number
- CN202410929194.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing jade adhesives have problems such as low bonding strength, easy misalignment, sensitivity to environmental changes, and excessively fast curing speed, making it difficult to meet the needs of jade cultural relic protection and restoration.
The light-cured jade adhesive is composed of difunctional (meth)acrylate monomers, diluent monomers, (meth)acrylate-type phosphates, photoinitiators, and co-initiators. It is cured by blue light or ultraviolet light to achieve a highly efficient and stable bonding process.
It improves the shear properties and bonding effect of jade adhesive, reduces the risk of misalignment of the bonding surface, enhances the stability to environmental changes, and is suitable for wetting and chemical reaction bonding of jade surfaces.
Smart Images

Figure BDA0004939139140000031 
Figure BDA0004939139140000051 
Figure BDA0004939139140000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of jade adhesives, and in particular relates to a light-cured jade adhesive and a preparation method and application thereof. Background Art
[0002] As a precious historical heritage of my country, jade cultural relics have extremely high research value. In recent years, with the large-scale excavation of jade cultural relics from the Neolithic Age, the demand for the protection and restoration of deteriorated jade has increased significantly, which has promoted scientific research in related directions. In the repair process of jade, the adhesive repair method, as one of the widely used and effective methods, has gradually attracted attention from the industry. The scope of application of traditional adhesive materials is limited due to the shortcomings of low bonding strength, poor mechanical properties, and low transparency. Modern adhesive materials can be divided into a variety of materials such as resin type, rubber type, and mixed solution type. Today, the commonly used jade adhesives are mainly epoxy resin glue and 502 instant glue, both of which have obvious defects. Epoxy resin glue requires external pressure during the bonding process, and the bonding surface is prone to displacement and dislocation. One of the defects of 502 instant glue is that it is sensitive to environmental changes and is prone to failure in a humid environment; the second defect is that it is volatile, and the volatilized gas has irritating odor and weak tear properties; the third defect is that the curing speed is too fast, and it is very easy to adhere to clothing and skin, which increases the difficulty of use. With the advancement of science and technology, adhesive materials have developed rapidly, and various new adhesive materials have come out one after another, bringing the methods of cultural relics protection and restoration into a new field. Summary of the invention
[0003] To overcome the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a light-cured jade adhesive.
[0004] Another object of the present invention is to provide a method for preparing the above-mentioned light-cured jade adhesive.
[0005] Another object of the present invention is to provide an application of the above-mentioned light-cured jade adhesive.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A light-cured jade adhesive, comprising the following components by weight:
[0008] 40-80 parts of difunctional or higher (meth)acrylate monomer, 20-60 parts of diluent monomer, 5-20 parts of (meth)acrylate secondary phosphate, 0.3-1.0 parts of photoinitiator, and 0.3-1.0 parts of co-initiator;
[0009] The relative molecular weight of the difunctional or higher (meth)acrylate monomer is ≥250 g / mol, and the viscosity is ≥10 CP; the relative molecular weight of the diluent is <250 g / mol, and the viscosity is <10 CP.
[0010] Preferably, the photocurable jade adhesive comprises the following components, measured by mass: 51 to 57 parts of difunctional or higher (meth)acrylate monomers, 34 to 38 parts of diluent monomers, 5 to 15 parts of (meth)acrylate type secondary phosphates, 0.3 to 1.0 parts of photoinitiators, and 0.3 to 1.0 parts of co-initiators.
[0011] Further preferably, the photocurable jade adhesive comprises the following components, calculated by weight: 51 to 57 parts of difunctional or higher (meth)acrylate monomers, 34 to 38 parts of diluent monomers, 5 to 10 parts of (meth)acrylate type secondary phosphates, 0.3 to 1.0 parts of photoinitiators, and 0.3 to 1.0 parts of co-initiators.
[0012] More preferably, the photocurable jade adhesive comprises the following components, calculated by weight: 54 to 57 parts of difunctional or higher (meth)acrylate monomers, 36 to 38 parts of diluent monomers, 5 to 10 parts of (meth)acrylate type secondary phosphates, 0.3 to 1.0 parts of photoinitiators, and 0.3 to 1.0 parts of co-initiators.
[0013] Most preferably, the photocurable jade adhesive comprises the following components, by mass: 54-57 parts of difunctional or higher (meth)acrylate monomers, 36-38 parts of diluent monomers, 5-10 parts of (meth)acrylate type secondary phosphates, 0.7 parts of photoinitiators, and 0.7 parts of co-initiators.
[0014] Preferably, the difunctional or higher (meth)acrylate monomer is at least one of difunctional or higher polyurethane (meth)acrylate, difunctional or higher epoxy resin (meth)acrylate, difunctional or higher bisphenol A (meth)acrylate and Bis-EFMA.
[0015] More preferably, the difunctional and / or multifunctional (meth)acrylate monomer is at least one of difunctional polyurethane (meth)acrylate and Bis-EFMA.
[0016] Still further preferably, the difunctional and / or multifunctional (meth)acrylate monomer is at least one of di(meth)acrylic acid urethane and Bis-EFMA.
[0017] Most preferably, the difunctional and / or multifunctional (meth)acrylate monomer is di(meth)acrylic acid urethane or a mixture of di(meth)acrylic acid urethane and Bis-EFMA in a mass ratio of 3:2.
[0018] The structural formula of the Bis-EFMA is as follows:
[0019]
[0020] Preferably, the diluent monomer is at least one of a reactive diluent monomer and a non-reactive diluent monomer; the reactive diluent is an unsaturated terminal olefin-containing monomer, including monofunctional, difunctional and polyfunctional unsaturated terminal olefin-containing monomers; more preferably, it is a (meth)acrylate monomer; most preferably, it is at least one of hydroxyethyl methacrylate, hydroxypropyl methacrylate and hydroxybutyl methacrylate; the non-reactive diluent monomer is an organic solvent; the organic solvent is at least one of toluene, ethanol and acetone.
[0021] Preferably, the (meth)acrylate type secondary phosphate is di[2-(methacryloyloxy)ethyl]phosphate.
[0022] Preferably, the photoinitiator is at least one of DL-camphorquinone, benzophenone and 1-phenyl-1,2-propanedione, more preferably DL-camphorquinone.
[0023] Preferably, the co-initiator is at least one of ethyl p-N,N-dimethylaminobenzoate and dimethylaminoethyl methacrylate, more preferably ethyl p-N,N-dimethylaminobenzoate.
[0024] The preparation method of the above-mentioned photocurable jade adhesive comprises the following steps: mixing bifunctional or higher (methyl)acrylate monomers, diluent monomers, (methyl)acrylate secondary phosphates, photoinitiators and co-initiators in proportion and in the dark to obtain a photocurable jade adhesive.
[0025] The above-mentioned photocuring jade adhesive is used in jade bonding.
[0026] Preferably, in the application, the light-cured jade adhesive is polymerized for 20 to 60 seconds under light irradiation for curing; the light is at least one of blue light and ultraviolet light; the light intensity range is 500 to 2000 mW / cm 2 .
[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0028] (1) The jade adhesive provided by the present invention only needs blue light curing during the bonding process, which is convenient and efficient. Different from the curing method of the existing jade adhesive, the jade adhesive of the present invention generally does not have the risk of dislocation of the bonding surface, is insensitive to environmental changes, and has a stable bonding effect.
[0029] (2) The jade adhesive formula provided by the present invention is composed of a difunctional or higher (methyl) acrylate monomer, a diluent monomer, a phosphate monomer, a photoinitiator and a co-initiator, which achieves an improvement in shear performance compared with existing adhesives.
[0030] (3) The jade adhesive provided by the present invention not only utilizes its own surface properties to wet the jade surface, but also utilizes the characteristic that the phosphate monomer can chemically react with the jade components to achieve bonding and repair of the broken surface of the jade, thereby enhancing the bonding effect and having good application prospects. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0032] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.
[0033] The raw materials of the photocurable jade adhesives provided in Examples 1 to 8 and Comparative Examples 1 to 3 are listed in Table 1 in parts by weight, wherein the diluent monomer is hydroxyethyl methacrylate, the photoinitiator is DL-camphorquinone, and the co-initiator is ethyl p-N,N-dimethylaminobenzoate.
[0034] Table 1 Mass composition table of Examples 1 to 6 and Comparative Examples 1 to 3 and 5 to 6
[0035]
[0036] The preparation process of jade adhesive is as follows:
[0037] (1) Add 0.05 mol of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (Bis-HEPF) and 0.1 mol of 2-(methacryloyloxy)ethyl isocyanate as reactants to a 250 ml round-mouth flask, then add a few drops of dibutyltin dilaurate as a catalyst and a small amount of 4-methoxyphenol as an inhibitor to the round-mouth flask, wherein the amount of the inhibitor is 0.5% of the total mass of the reactants, and finally add acetone as a solvent, stir at room temperature, and dissolve all the substances in acetone. Place the round-bottom flask in an oil bath and heat it at 43 degrees, and turn on the magnetic stirrer to react for 36 hours. After the reaction is completed, take a sample of the liquid in the round-mouth flask for Fourier infrared spectroscopy test to detect whether the sample has an absorption peak of the -NCO group at 2270 wavenumbers. If there is an absorption peak, the reaction is continued for a longer time; if there is no absorption peak, the reaction is terminated and post-processing is performed.
[0038] (2) The removed round-mouth flask is placed on a rotary evaporator and heated in a water bath at 70 degrees. The round-mouth flask is periodically removed and weighed during the heating period until the acetone is completely evaporated, and the rotary evaporation is terminated. The sample is taken out and the obtained product is Bis-EFMA.
[0039] (3) Accurately weigh the raw material components shown in Table 1 into a brown bottle, and wrap the outside of the brown bottle with aluminum foil to protect it from light. Add a magnet into the bottle and stir it at room temperature for 12 hours to obtain a blue light-induced jade adhesive.
[0040] The chemical equations for the above reaction steps are shown below:
[0041]
[0042] Comparative Example 4: Commercially available product 502 instant adhesive
[0043] In order to illustrate that the blue light-cured jade adhesive described in the present invention has the advantage of improving shear strength, the commercially available product 502 instant adhesive is used as comparative example 4.
[0044] The characterization methods used for Examples 1 to 8 and Comparative Example 1 are as follows:
[0045] 1. Double bond conversion rate test of jade adhesive samples: Double bond conversion rate is an experiment to determine the degree of chemical reaction of double bonds in a material within a specified time.
[0046] The sample to be tested is evenly spread into a thin film on a potassium bromide sheet. Record the infrared spectrum of the sample before curing; then use a blue light curing lamp to cure the sample at room temperature for 40 seconds, and then record the infrared spectrum of the sample after curing. Because the stretching vibration peak intensity of the C=C double bond at 1640 wavenumbers is significantly reduced before and after blue light irradiation, while the characteristic peak of the benzene ring at 1608 wavenumbers has no obvious change. Therefore, the infrared spectrum is normalized with the characteristic absorption peak of the benzene ring at 1608 wavenumbers as the internal standard peak, and the double bond conversion rate (DC) is calculated based on the change in the absorption peak of the C=C double bond at 1636 wavenumbers before and after the sample is cured. Each group of samples is measured 6 times, and the arithmetic mean of the 6 results of each group is taken as the final result of the sample. The calculation formula is shown in (1):
[0047]
[0048] In the formula, A C=C and A ph are the infrared spectrum absorption peak areas of the sample at the C=C double bond at 1640 wavenumber and the benzene ring at 1608 wavenumber; (A C=C / A ph ) t and (A C=C / A ph )0 represents the normalized absorption peak intensity of C=C double bond at t seconds and 0 seconds of illumination. DC is the double bond conversion rate of the sample when the blue light is irradiated for t seconds.
[0049] The test results are shown in Table 2.
[0050] 2. Test of flexural strength and flexural elastic modulus of jade adhesive samples: The flexural performance test is an experiment to determine the mechanical properties of a material when it is subjected to a bending load. Currently, the three-point bending method is commonly used for bending experiments on resins.
[0051] With polyester film as the substrate, the sample was injected into a rectangular silicone mold with a size of 25 mm × 2 mm × 2 mm, and then covered with polyester film to flatten and expel bubbles; the sample was evenly divided into five equal parts, and each part of the sample was irradiated with a blue light curing lamp for 40 seconds, and then the cured specimen was taken out. After the specimen was cured, it was polished with a metallographic specimen grinder (grinding disc diameter 230 mm, speed 180 rpm). Six specimens were prepared for each specimen, and the arithmetic mean of the six specimens in each group was taken as the final result of the specimen.
[0052] The test was carried out using a universal material testing machine, with the load rate set to 1.00 mm / min and the spline span set to 20 mm. The flexural strength (FS) and flexural modulus (FM) of the spline were calculated using formulas (2) and (3) respectively:
[0053]
[0054] Where F is the load, l is the span, b is the width, and h is the thickness.
[0055]
[0056] Where σ is stress and ε is strain.
[0057] The test results are shown in Table 3.
[0058] 3. Surface contact angle test of jade adhesive on jade: Surface contact angle is an experiment to measure the wettability of a material on a specified surface.
[0059] First, the jade was embedded with resin, and the prepared sample tables were divided into two groups. Then, they were polished in groups using 500-mesh and 2000-mesh sandpapers. Each polished sample table was ultrasonically cleaned in anhydrous ethanol for 30 minutes to remove the abrasive materials that may be embedded on the surface of the sample table. After the ultrasonic treatment, the sample tables were placed in a dryer to dry for later use.
[0060] Use a disposable syringe to absorb an appropriate amount of sample and drop it on the surface of the sample table. After the droplet is stable on the surface of the sample table for 20 seconds, measure the surface contact angle of the sample. Each group of samples is measured 6 times, and the arithmetic mean of the 6 results of each group is taken as the final result.
[0061] The test results are shown in Table 4.
[0062] 4. Shear strength test of jade adhesive samples: The shear performance test is an experiment to determine the maximum load that the bonded parts can withstand per unit area parallel to the bonding surface. It is an important indicator of the bonding strength of the adhesive.
[0063] First, the jade was embedded with resin to prepare the sample table, and an appropriate amount of sample was applied to the sample table after being polished with 500-mesh and 2000-mesh sandpaper, respectively, and the jade was contacted with the sample table. The sample preparation was completed after the 4 groups of comparative examples were left in the air for 40 seconds, and the sample preparation was completed after the other groups of samples were irradiated with a blue light at the bonding point for 40 seconds. The number of sample tables tested in each group was 6, and the arithmetic average of the 6 measurement results of each group was taken as the final result.
[0064] The test was carried out using a universal material testing machine, with the load rate set at 1.00 mm / min. The shear strength (SS) of the specimen was calculated using formula (4):
[0065]
[0066] Where F is the load and d is the diameter of the jade.
[0067] The test results are shown in Table 5.
[0068] Table 2 Double bond conversion rate of jade adhesive samples after blue light curing for 40 seconds
[0069]
[0070]
[0071] Table 3 Flexural strength and flexural elastic modulus of jade adhesive samples
[0072]
[0073] Table 4 Surface contact angle of jade adhesive on jade
[0074]
[0075] Table 5 Shear strength of jade adhesive samples
[0076]
[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A light-cured jade adhesive, characterized in that: By mass, it includes the following components: 40-80 parts of difunctional or higher (meth)acrylate monomer, 20-60 parts of diluent monomer, 5-20 parts of (meth)acrylate secondary phosphate, 0.3-1.0 parts of photoinitiator, and 0.3-1.0 parts of co-initiator; The relative molecular weight of the difunctional or higher (meth)acrylate monomer is ≥250 g / mol, and the viscosity is ≥10 CP; the relative molecular weight of the diluent is <250 g / mol, and the viscosity is <10 CP.
2. A light-cured jade adhesive according to claim 1, characterized in that, The composition comprises the following components in parts by mass: 51 to 57 parts of difunctional or higher (meth)acrylate monomers, 34 to 38 parts of diluent monomers, 5 to 15 parts of (meth)acrylate type secondary phosphates, 0.3 to 1.0 parts of photoinitiators, and 0.3 to 1.0 parts of co-initiators.
3. A light-cured jade adhesive according to claim 2, characterized in that, The composition comprises the following components in parts by mass: 51 to 57 parts of difunctional or higher (meth)acrylate monomers, 34 to 38 parts of diluent monomers, 5 to 10 parts of (meth)acrylate type secondary phosphates, 0.3 to 1.0 parts of photoinitiators, and 0.3 to 1.0 parts of co-initiators.
4. A light-cured jade adhesive according to claim 3, characterized in that: The composition comprises the following components in parts by mass: 54-57 parts of difunctional or higher (meth)acrylate monomers, 36-38 parts of diluent monomers, 5-10 parts of (meth)acrylate type secondary phosphates, 0.3-1.0 parts of photoinitiators, and 0.3-1.0 parts of co-initiators.
5. A light-cured jade adhesive according to claim 1, characterized in that: The (meth)acrylate type secondary phosphate is di[2-(methacryloyloxy)ethyl]phosphate.
6. A light-cured jade adhesive according to claim 1, characterized in that: The difunctional or higher (meth)acrylate monomer is at least one of difunctional or higher polyurethane (meth)acrylate, difunctional or higher epoxy resin (meth)acrylate, difunctional or higher bisphenol A (meth)acrylate and Bis-EFMA; The diluent monomer is at least one of a reactive diluent monomer and a non-reactive diluent monomer; the reactive diluent is a monomer containing an unsaturated terminal olefin group; the non-reactive diluent monomer is an organic solvent; The structural formula of the Bis-EFMA is as follows:
7. A light-cured jade adhesive according to claim 6, characterized in that: The difunctional and / or multifunctional (meth)acrylate monomer is at least one of difunctional polyurethane (meth)acrylate and Bis-EFMA; Or, the difunctional and / or multifunctional (meth)acrylate monomer is at least one of di(meth)acrylic acid urethane and Bis-EFMA; The reactive diluent is a (meth)acrylate monomer; or the reactive diluent is at least one of hydroxyethyl methacrylate, hydroxypropyl methacrylate and hydroxybutyl methacrylate; The organic solvent is at least one of toluene, ethanol and acetone.
8. A light-cured jade adhesive according to claim 1, characterized in that: The photoinitiator is at least one of DL-camphorquinone, benzophenone and 1-phenyl-1,2-propanedione; The auxiliary initiator is at least one of ethyl p-N,N-dimethylaminobenzoate, ethyl dimethylaminobenzoate and dimethylaminoethyl methacrylate.
9. A method for preparing a light-cured jade adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: The (meth)acrylate monomer with difunctionality or above, the diluent monomer, the (meth)acrylate type secondary phosphate, the photoinitiator and the auxiliary initiator are mixed evenly in proportion in the dark to obtain a light-cured jade adhesive.
10. Use of a light-cured jade adhesive according to any one of claims 1 to 8 in jade bonding, characterized in that: The adhesive cures under exposure to blue light and / or UV light.
Citation Information
Patent Citations
Stone surface treatment agent and preparation method thereof and stone surface treatment method
CN110511653A
Adhesive for optical disk and optical disk
CN1531726A
Adhesive composition
JP1987236877A
Photocurable resin composition
JP1998287718A
Photocurable resin composition
WO1998036325A1
Cited By
Multi-component hybrid siloxane, preparation thereof and application of multi-component hybrid siloxane in jade cultural relic protection
CN120349514A