Preparation method of nickel-based high-temperature alloy GH4169
Through a multi-step process, including aluminum thermal reaction, electroslag remelting and forging, the composition segregation and pore problems of nickel-based high-temperature alloy GH4169 are solved, significantly improving its element distribution uniformity and stability, and reducing the " The emergence of dark spots and pores improves the performance of the alloy.
Patent Information
- Application Number
- CN202411037304.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-05
AI Technical Summary
During the preparation process, the nickel-based high-temperature alloy GH4169 has problems with component segregation, uneven element distribution, pores and shrinkage, resulting in cracks and abnormal fractures in the parts during use.
Using a process flow including primary mixing, aluminum thermal reaction, crushing and remixing, initial melting, electroslag remelting, forging, heat treatment and three melting, the melting point of high melting point elements is reduced by aluminum thermal method, and the electroslag heavy is reduced by Melting reduces non-metallic impurities, forging and pressing improves grain structure, and vacuum consumable arc furnaces improves element distribution uniformity.
It significantly reduces the composition segregation, macroscopic segregation and pore problems of the alloy, improves the uniformity of element distribution, enhances the stability and performance of the alloy, and reduces the appearance of "black spots", "white spots" and pores.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy processing, and in particular to a preparation method of a nickel-based high-temperature alloy GH4169. Background Art
[0002] Nickel-based superalloy GH4169 is a Nb-strengthened Ni-Cr-Fe-based precipitation-hardening deformation superalloy with high yield strength, tensile strength, toughness, plasticity, fatigue life and creep resistance below 650°C. It is widely used in aviation, aerospace, nuclear energy, petrochemical and other fields. Its long-term use temperature range is -253 to 650°C, and its short-term use temperature can reach 800°C. The turbine disks, casings, fasteners, elastic elements, damping elements and other parts made of it have been used in aircraft engines for a long time. At present, GH4169 has become the largest, most widely used, and most complete product variety and specification deformation superalloy material in various types of aircraft engines currently in service and under development in my country.
[0003] When the nickel-based high-temperature alloy GH4169 is prepared by the smelting method, there are one-time smelting method, two-way smelting method, and three-way smelting method. Generally, there are more problems caused by one-time smelting, especially the nickel-based high-temperature alloy GH4169 contains high-melting point elements such as Cr, Mo, and Nb. These high-melting point elements have different melting points and densities. When each single substance is used as an electrode block to melt the nickel-based high-temperature alloy GH4169, the melting rate of each raw material is also different, which causes some metals to overheat, further causing alloy component segregation and high-density inclusions. At the same time, the alloy made by one-time smelting has a high content of hazardous elements such as nitrogen, oxygen, and sulfur. These defects cause certain metallurgical defects in the castings of the nickel-based high-temperature alloy GH4169, which will cause crack sources due to inclusions or segregation, thereby causing abnormal fractures when the parts are in service. The three-way smelting process, namely VIM+ESR+(VIM or VAR), is used to prepare the nickel-based high-temperature alloy GH4169, which has a better effect. The content of harmful elements such as nitrogen, oxygen, and sulfur is low, and the problems of alloy component segregation and high-density inclusions have been improved to a certain extent. However, affected by the production raw materials and the smelting process itself, the nickel-based high-temperature alloy GH4169 is still prone to obvious macroscopic segregation and dendrite segregation in some parts, and "black spots" and "white spots" appear on the alloy surface. At the same time, there are too many pores inside the alloy, which will affect the use of the alloy. Summary of the invention
[0004] In view of this, it is necessary to provide a preparation method of a nickel-based high-temperature alloy GH4169 which reduces alloy component segregation, has more uniform element distribution, and has fewer pores and shrinkage problems.
[0005] A method for preparing a nickel-based high-temperature alloy GH4169 comprises the following steps:
[0006] Step S1: initial mixing; the following raw materials are proportioned and mixed according to weight percentage to form a primary mixture, wherein metal nickel powder: chromium oxide: niobium oxide: molybdenum oxide: aluminum powder: calcium fluoride: calcium oxide: potassium chlorate = 0.07-0.2: 0.05-0.15: 0.2-0.4: 0.15-0.2: 0.2-0.4: 0-0.07: 0-0.30: 0.02-0.05;
[0007] Step S2: smelting the master alloy; placing the primary mixed material into the furnace of a vacuum reactor for aluminothermic reaction, cooling it to form a master alloy and taking it out of the furnace;
[0008] Step S3: secondary mixing; crushing the master alloy into particles with a particle size less than or equal to 10 cm, and mixing with nickel, chromium, aluminum, titanium, and carbon to form a remix, wherein the mass ratio of nickel, chromium, aluminum, titanium, carbon, iron, and master alloy is (94±3):(36±2):(1±0.2):(2±0.2):(0.07-0.15):(36±1):(32±1);
[0009] Step S4: initial melting; pouring the remixed material into an induction vacuum furnace for initial melting of the GH4169 alloy to form an initial melt alloy;
[0010] Step S5: remelting; electroslag remelting the primary molten alloy, cooling the molten metal in the molten pool to 980-1050 degrees Celsius, and keeping the temperature for 30-40 minutes to obtain a secondary molten alloy, wherein the slag contains aluminum powder, and the mass ratio of the aluminum powder to the slag is 0.5-1%;
[0011] Step S6: forging; forging the second melt alloy in a forging press, with a pass deformation of 25 to 33%, to obtain a primary forged alloy ingot;
[0012] Step S7: heat treatment; heating the two melts of the alloy to 940-980 degrees Celsius in a vacuum electric heating furnace, and keeping the temperature for 1-1.5 hours, and then cooling to room temperature at a rate of 55-75 degrees Celsius per minute to form a heat-treated alloy ingot;
[0013] Step S8: three-time smelting: smelting the heat-treated alloy ingot three times in a vacuum consumable arc furnace, and obtaining the nickel-based high-temperature alloy GH4169 of the present invention after cooling.
[0014] Beneficial effects: Compared with the prior art, the nickel-based high-temperature alloy GH4169 prepared by the preparation method of the present invention has more uniform alloy composition, better component segregation, less macroscopic segregation, less dendrite segregation, and fewer problems such as "white spots" and "black spots". At the same time, the alloy has fewer problems such as pores and shrinkage holes. DETAILED DESCRIPTION
[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the following description is about some embodiments of the present invention.
[0016] The preparation method of nickel-based high temperature alloy GH4169 comprises the following steps:
[0017] Step S1: initial mixing; the following raw materials are proportioned and mixed according to weight percentage to form a primary mixture, wherein metal nickel powder: chromium oxide: niobium oxide: molybdenum oxide: aluminum powder: calcium fluoride: calcium oxide: potassium chlorate = 0.07-0.2: 0.05-0.15: 0.2-0.4: 0.15-0.2: 0.2-0.4: 0-0.07: 0-0.30: 0.02-0.05;
[0018] Step S2: smelting the master alloy; placing the primary mixed material into the furnace of a vacuum reactor for aluminothermic reaction, cooling it to form a master alloy and taking it out of the furnace;
[0019] The smelting process of the master alloy is to use the aluminothermic method to cause a uniformly mixed metal oxide to undergo an oxidation-reduction reaction with aluminum to generate each metal element. Since it is in a mixed state and the high temperature generated by the heat release during the reaction is sufficient to melt the metal, the mixture forms an alloy after the aluminothermic reaction. At the same time, the density of the replaced aluminum oxide is relatively small, and most of the aluminum will float on the surface of the melt and fall off as slag after cooling. The temperature of the aluminothermic method is very high, which can quickly melt the high-melting-point elements and mix them evenly. At the same time, preparing the master alloy and then mixing and smelting can also reduce the heat loss during the subsequent initial melting.
[0020] The intermediate alloy melts high-melting-point chromium, molybdenum, niobium and part of low-melting-point nickel to reduce the melting point of the subsequent GH4169 alloy raw material melting. In this way, the high-melting-point metal is in an alloy state during the subsequent melting process and can be melted at a lower temperature, thereby being more evenly mixed with other elements and significantly improving the phenomenon of component segregation.
[0021] Step S3: secondary mixing; crushing the master alloy into particles with a particle size less than or equal to 10 cm, and mixing with nickel, chromium, aluminum, titanium, and carbon to form a remix, wherein the mass ratio of nickel, chromium, aluminum, titanium, carbon, iron, and master alloy is (94±3):(36±2):(1±0.2):(2±0.2):(0.07-0.15):(36±1):(32±1);
[0022] Step S4: initial melting; pouring the remixed material into an induction vacuum furnace for initial melting of the GH4169 alloy to form an initial melt alloy;
[0023] The primary melting is mainly to preliminarily melt the crushed intermediate alloy and the remaining metal element to form the primary melting alloy of GH4169 alloy. After the primary melting, the primary melting alloy ingot is poured out from the furnace body after cooling and shaping and used as the consumable electrode of the electroslag furnace for secondary melting, in order to obtain an alloy with less non-metal content and less segregation problems. Specifically, as shown in step S5.
[0024] Step S5: remelting; electroslag remelting the primary molten alloy, cooling the molten metal in the molten pool to 980-1050 degrees Celsius, and keeping the temperature for 30-40 minutes to obtain a secondary molten alloy, wherein the slag contains aluminum powder, and the mass ratio of the aluminum powder to the slag is 0.5-1%;
[0025] Through experiments, it is found that keeping the temperature within the range of 980 to 1050 degrees Celsius for 30 to 40 minutes can properly and stably develop the grains inside the alloy, improve the uniformity of the grain size, and make the alloy have good brittleness, which is convenient for destroying the grain and dendrite structure during the forging process. The forging process is as step S6.
[0026] Step S6: forging; forging the second melt alloy in a forging press, with a deformation amount of 25 to 33% per pass, to obtain a primary forged alloy ingot; the forging can be performed in an alternating manner of upsetting and drawing.
[0027] At the beginning of forging, the alloy temperature is maintained at 980-1050 degrees Celsius. During the forging process, due to the large deformation of each pass, very large stress is generated inside the alloy. At the same time, the alloy temperature is high, the large grains in the alloy are more easily destroyed, the grain structure is more uniform, and the dendrites are more likely to break, making the distribution of elements inside the alloy more uniform, which is convenient for improving the stability of the smelting process in the subsequent three smeltings.
[0028] At the same time, the electroslag melting process will cause the alloy to produce more pores, shrinkage holes, etc., especially on the surface of the alloy. If not treated, in the subsequent three melting processes, these gaps may fall into the molten pool along with the solid matter that has not had time to melt, so that the alloy will still have pores and shrinkage holes after cooling, thus affecting the alloy performance. The pores and shrinkage holes on the surface of the alloy can be significantly improved by forging. At the same time, under the action of extrusion, the shrinkage hole problem inside the alloy can also be improved, so that the pores on the surface of the second-melt alloy will not enter the interior of the final alloy ingot.
[0029] After forging, the alloy temperature is naturally cooled to below 200 degrees Celsius, and then the alloy is heat treated. The heat treatment process is as step S5.
[0030] Step S7: heat treatment; heating the two melts of the alloy to 940-980 degrees Celsius in a vacuum electric heating furnace, and keeping the temperature for 1-1.5 hours, and then cooling to room temperature at a rate of 55-75 degrees Celsius per minute to form a heat-treated alloy ingot;
[0031] The heat treatment process is mainly to improve the internal grain structure of the second-melt alloy, make the grains finer, and make the subsequent alloy melting more stable and thorough, preventing a small amount of alloy from falling into the molten pool without melting.
[0032] Step S8: three-time smelting: smelting the heat-treated alloy ingot three times in a vacuum consumable arc furnace, and obtaining the nickel-based high-temperature alloy GH4169 of the present invention after cooling.
[0033] The vacuum consumable arc furnace has an electromagnetic stirring effect on the molten liquid in the molten pool, so that the elements in the molten liquid are more evenly distributed. At the same time, during the stirring process, the stratification of metals with different densities is slower, and the segregation of the alloy after cooling is lighter.
[0034] The present invention replaces the high melting point metal oxide in the raw material with a single substance by the aluminothermic method, and can melt and form an alloy by utilizing the heat released by the aluminothermic reaction under the condition of less heat energy supply, thereby reducing the consumption of heat energy. Moreover, the temperature of the heat release process of the aluminothermic method is very high, which can fully reach the melting point of each metal and heat up rapidly, which is beneficial to improving the uniformity of the alloy components and reducing component segregation. Affected by the uncontrolled temperature of the aluminothermic method and the uneven mixing of raw materials, the component uniformity of the intermediate alloy is poor. At the same time, the oxygen content of the intermediate alloy produced by the aluminothermic method is higher than that of the nickel-based high-temperature alloy GH4169 obtained by other methods. The present invention mixes the intermediate alloy with other metal components in a vacuum induction furnace to form a primary melt alloy. The oxygen content in the intermediate alloy is removed by carbon elements, thereby reducing the content of oxygen elements in the alloy. Then, the secondary melt alloy is obtained by electroslag remelting. The electroslag contains a small amount of aluminum powder. When the alloy melt passes through the electroslag, the oxides in the melt can react with the aluminum powder. At the same time, the non-metallic impurities in the alloy will be dissolved in the slag. After electroslag remelting, the non-metal content in the alloy can be effectively reduced. The alkaline substances in the electroslag can effectively absorb sulfur, and the nitrogen, oxygen, and sulfur contents in the alloy are significantly reduced. At the same time, electroslag remelting can fully melt the alloy. In this process, the alloy melts to form droplets and enters the molten pool. The elements in the droplets will be redistributed, and the element concentration problem in the local area of the alloy can be effectively alleviated. Despite this, after testing, the nickel-based high-temperature alloy GH4169 will still have problems such as intracrystalline segregation and dendrite segregation after electroslag remelting. The present invention destroys the grain structure in the alloy ingot by forging the two-melt alloy, and then improves the grain structure through further heat treatment, so that the grain size, grain composition, etc. are more uniform. After that, the alloy is melted three times in a vacuum consumable arc furnace. During the alloy melting process, the grain size and grain composition are more uniform, making the melting process more stable. At the microscopic level, the element distribution during the remelting process is more uniform, making the nucleation process more uniform during the melting recrystallization process. There are fewer problems such as dendrite segregation and intracrystalline segregation.
[0035] In a preferred embodiment, the processing of the master alloy raw material in step S1 includes the following steps:
[0036] Step S101: drying chromium oxide, molybdenum oxide, niobium oxide, and calcium fluoride to remove moisture;
[0037] Step S102: calcining calcium oxide at a high temperature of 1000°C.
[0038] In a preferred embodiment, in step S2, the bottom of the furnace body of the vacuum reactor is paved with at least 5 mm of high-alumina refractory material with a mesh size of -100 to -40.
[0039] In a preferred embodiment, in step S2, after the mixture is prepared in the reactor, it is sealed and evacuated. When the vacuum degree is less than 0.5 MPa, the evacuation is stopped and argon is filled to a slightly positive pressure, and then the mixture is evacuated again until the vacuum degree is less than or equal to 0.5 MPa, and the argon filling and evacuation are repeated three times.
[0040] In a preferred embodiment, in step S3, the slag in the electroslag remelting includes calcium oxide, calcium fluoride, silicon dioxide, aluminum oxide, and aluminum.
[0041] In order to verify the effect of preparing the nickel-based high-temperature alloy GH4169 by the present invention, the present invention compares the widely used triple smelting method to prepare the GH4169 alloy, respectively detects the number and area of "white spots" and "black spots" of the prepared nickel-based high-temperature alloy GH4169, and samples and detects the composition content of the alloy at different positions of the GH4169 alloy ingot to compare the significance of component segregation. At the same time, the volume of pores and shrinkage cavities of the GH4169 alloy is also detected by flaw detection to verify the implementation effect of the present invention.
[0042] Embodiment 1: The GH4169 alloy is prepared by adopting the preparation method of the nickel-based high-temperature alloy GH4169 of the present invention.
[0043] The raw materials were proportioned and mixed according to the weight percentages in Table 1 to form a primary mixture, and then an intermediate alloy was prepared by aluminothermic method.
[0044] Table 1: Raw material ratio of master alloy
[0045]
[0046] The master alloy is crushed into particles with a particle size of less than 10 cm and mixed with nickel, chromium, aluminum, titanium, iron and carbon. The mass of each component is shown in Table 2.
[0047] Table 2: Raw material ratio of GH4169 alloy
[0048] Add to Weight kg Ni 94.2 Cr 34.1 Nb 0 Mo 0 Al 1 Ti 2 C 0.15 Fe 36 Master Alloy 32.7
[0049] The remixed material is poured into an induction vacuum furnace for the initial smelting of the GH4169 alloy to form a primary melt alloy; the primary melt alloy is electroslag remelted, and the molten metal in the molten pool is cooled to 980-1050 degrees Celsius and kept warm for 30-40 minutes to obtain a secondary melt alloy, wherein the slag contains aluminum powder, and the mass ratio of the aluminum powder to the slag is 0.5-1%; the secondary melt alloy is forged under a forging press, and the pass deformation is 25-33% to obtain a primary forged alloy ingot; the secondary melt alloy is heated to 940-980 degrees Celsius in a vacuum electric heating furnace, and kept warm for 1-1.5 hours, and then cooled to room temperature at a rate of 55-75 degrees Celsius per minute to form a heat-treated alloy ingot; the heat-treated alloy ingot is smelted three times in a vacuum consumable arc furnace, and the nickel-based high-temperature alloy GH4169 of the present invention is obtained after cooling.
[0050] Example 2: GH4169 alloy was prepared by triple smelting method.
[0051] The raw materials were mixed according to the weight percentages in Table 3.
[0052] Table 3: Raw material ratio of GH4169 alloy prepared by triple smelting method
[0053]
[0054]
[0055] The raw materials are first poured into a vacuum induction furnace for primary smelting to obtain a primary molten alloy; the primary molten alloy is then electroslag remelted to obtain a secondary molten alloy; finally, the secondary molten alloy is smelted three times in a vacuum consumable arc furnace, and the GH4169 alloy is obtained after cooling. This method is a conventional method in the art, and therefore, the various parameters in the process will not be described in detail.
[0056] The black spots, white spots, pores and shrinkage cavities of the GH4169 alloy prepared in Example 1 and Example 2 are shown in Table 4.
[0057] Table 4:
[0058] Number of black spots Total area of black spots Number of white spots Total white spot area Total volume of pores and shrinkage cavities Embodiment 1 2 places <![CDATA[2.3cm 2 ]]> 1 place <![CDATA[0.6cm 2 ]]> <![CDATA[0.07cm 3 ]]> Embodiment 2 6 places <![CDATA[10.1cm 2 ]]> 4 places <![CDATA[7.3cm 2 ]]> <![CDATA[0.18cm 3 ]]>
[0059] As can be seen from Table 4, the number of black spots in Example 1, that is, the GH4169 alloy prepared by the present invention, is only two, which is significantly less than the six black spots in Example 2, which is prepared by the triple smelting method. At the same time, the total area of the black spots in Example 1 is only one-fourth of that in Example 2, and the black spot phenomenon is significantly improved. At the same time, the number and total area of white spots in Example 1 are also significantly lower than those in Example 2. In terms of pores and shrinkage cavities, the total volume of pores and shrinkage cavities in Example 1 is only 0.07 cm 3, while the total volume of pores and shrinkage holes in Example 2 is 0.18 cm 3 , which is close to three times that of Example 1. The GH4169 alloy prepared by the present invention is also significantly improved in terms of pores and shrinkage holes.
[0060] At the same time, the composition segregation and dendrite segregation of Example 1 and Example 2 are also tested, and the specific process is as follows:
[0061] Cut the alloy ingot horizontally into two parts along the middle position. Take three points a1, b1, and c1 on the diagonal line of the upper surface of the upper alloy ingot for sampling and analysis. The middle point is located at the center of the upper surface, and the points on both sides are located at the edge of the upper surface. Similarly, take three points a2, b2, and c2 at the same position on the lower surface of the upper alloy ingot for sampling and analysis; take three points a3, b3, and c3 at the same position on the lower surface of the lower alloy ingot for sampling and analysis. The composition detection results of the 9 sample points in Example 1 and Example 2 are shown in Tables 5 and 6:
[0062] Table 5: Statistics of percentage of each component in Example 1
[0063] Nb(%) Cr(%) Ni(%) Mo(%) Al(%) Ti(%) Fe(%) <![CDATA[a1]]> 4.97 19.2 51.5 2.99 0.56 0.93 36.1 <![CDATA[b1]]> 4.95 18.8 50.6 2.98 0.58 0.94 36.3 <![CDATA[c1]]> 4.98 19.2 50.9 2.96 0.57 0.89 36.4 <![CDATA[a2]]> 5.02 19.3 51.8 3.02 0.58 0.94 35.9 <![CDATA[b2]]> 5.04 18.9 51.7 3.01 0.56 0.96 35.8 <![CDATA[c2]]> 5.04 19.3 51.7 3.02 0.58 0.94 36.0 <![CDATA[a3]]> 5.07 19.0 51.8 3.04 0.55 0.95 35.7 <![CDATA[b3]]> 5.09 18.9 51.9 3.03 0.58 0.88 35.7 <![CDATA[c3]]> 5.06 19.1 51.8 3.04 0.57 0.94 35.6 average value 5.02 19.1 51.5 3.01 0.57 0.93 35.9 variance 0.002 0.034 0.21 0.0008 0.0001 0.0007 0.0778
[0064] Note: The influence of non-metallic elements on the results of composition segregation and dendrite segregation is negligible, so they are no longer counted in the table.
[0065] Table 6: Statistics of percentage of each component in Example 2
[0066] Nb(%) Cr(%) Ni(%) Mo(%) Al(%) Ti(%) Fe(%) <![CDATA[a1]]> 4.83 19.8 52.1 2.97 0.78 0.78 35.1 <![CDATA[b1]]> 4.91 19.6 52.3 2.95 0.79 0.79 35.3 <![CDATA[c1]]> 4.89 19.5 52.4 2.98 0.78 0.79 35.4 <![CDATA[a2]]> 4.96 20.3 52.3 3.02 0.77 0.81 35.7 <![CDATA[b2]]> 5.02 20.1 52.6 3.01 0.74 0.80 35.6 <![CDATA[c2]]> 5.04 20.1 52.5 3.02 0.74 0.82 35.6 <![CDATA[a3]]> 5.10 21.3 52.6 3.05 0.75 0.83 35.7 <![CDATA[b3]]> 5.09 20.9 52.4 3.06 0.76 0.82 35.8 <![CDATA[c3]]> 5.12 20.8 52.5 3.06 0.73 0.83 36.1 average value 5.00 20.3 52.4 3.01 0.76 0.81 35.6 variance 0.01 0.383 0.026 0.0016 0.0005 0.003 0.086
[0067] Note: The influence of non-metallic elements on the results of composition segregation and dendrite segregation is negligible, so they are no longer counted in the table.
[0068] It can be seen from the data in Tables 5 and 6 that the variances of Nb, Cr, and Mo in Example 1 are significantly reduced, indicating that the composition of the GH4169 alloy prepared by the present invention is significantly more uniform, especially for elements with high melting points, the problem of component segregation is significantly improved. At the same time, by observing the metallographic structure of 9 sampling points, the GH4169 alloy in Example 1 has a dendrite segregation problem, while the GH4169 alloy in Example 2 has three dendrite segregation problems, which shows that the preparation method of the nickel-based high-temperature alloy GH4169 of the present invention can also significantly improve the problem of dendrite segregation.
[0069] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A method for preparing a nickel-based high-temperature alloy GH4169, characterized in that: The following steps are involved: Step S1: initial mixing; the following raw materials are proportioned and mixed according to weight percentage to form a primary mixture, wherein metal nickel powder: chromium oxide: niobium oxide: molybdenum oxide: aluminum powder: calcium fluoride: calcium oxide: potassium chlorate = 0.07~0.2: 0.05~0.15: 0.2~0.4: 0.15~0.2: 0.2~0.4: 0~0.07: 0~0.30: 0.02-0.05; Step S2: smelting the master alloy; placing the primary mixed material into the furnace of a vacuum reactor for aluminothermic reaction, cooling it to form a master alloy and taking it out of the furnace; Step S3: secondary mixing; crushing the master alloy into particles with a particle size less than or equal to 10 cm, and mixing with nickel, chromium, aluminum, titanium, and carbon to form a re-mixed material, wherein the mass ratio of nickel, chromium, aluminum, titanium, carbon, iron, and master alloy is (94±3): (36±2): (1±0.2): (2±0.2): (0.07-0.15): (36±1): (32±1); Step S4: initial melting; pouring the remixed material into an induction vacuum furnace for initial melting of the GH4169 alloy to form an initial melt alloy; Step S5: remelting; electroslag remelting the primary molten alloy, cooling the molten metal in the molten pool to 980-1050 degrees Celsius and keeping the temperature for 30-40 minutes to obtain a secondary molten alloy, wherein the slag contains aluminum powder, and the mass ratio of the aluminum powder to the slag is 0.5-1%; Step S6: forging; forging the second melt alloy in a forging press, with a pass deformation of 25-33%, to obtain a primary forged alloy ingot; Step S7: heat treatment; heating the two melts of the alloy to 940-980 degrees Celsius in a vacuum electric heating furnace, and keeping the temperature for 1-1.5 hours, and then cooling the temperature to room temperature at a rate of 55-75 degrees Celsius per minute to form a heat-treated alloy ingot; Step S8: three-time smelting: smelting the heat-treated alloy ingot three times in a vacuum consumable arc furnace, and obtaining the nickel-based high-temperature alloy GH4169 of the present invention after cooling.
2. The method for preparing the nickel-based high-temperature alloy GH4169 according to claim 1, characterized in that: In step S1, the processing of the master alloy raw material includes the following steps: Step S101: drying chromium oxide, molybdenum oxide, niobium oxide, and calcium fluoride to remove moisture; Step S102: calcining calcium oxide at a high temperature of 1000°C.
3. The method for preparing the nickel-based high-temperature alloy GH4169 according to claim 1, characterized in that: In step S2, the bottom of the furnace body of the vacuum reaction furnace is paved with -100 mesh to -40 mesh high-alumina refractory material with a thickness of at least 5 mm.
4. The method for preparing the nickel-based high-temperature alloy GH4169 according to claim 1, characterized in that: In step S2, after the mixture is prepared in the reactor, it is sealed and evacuated. When the vacuum degree is less than 0.5 MPa, the evacuation is stopped and argon is filled to a slightly positive pressure, and then the mixture is evacuated again until the vacuum degree is less than or equal to 0.5 MPa. The argon filling and evacuation process is repeated three times.
5. The method for preparing the nickel-based high-temperature alloy GH4169 according to claim 1, characterized in that: In step S5, the slag in the electroslag remelting includes calcium oxide, calcium fluoride, silicon dioxide, aluminum oxide, and aluminum.