Heat-resistant and corrosion-resistant magnesium alloy and preparation method thereof

Through multi-component alloying and specific heat treatment technology, the problems of poor high-temperature mechanical and corrosion resistance of magnesium alloys are solved, the performance improvement and cost reduction of magnesium alloys are achieved, and the heat-resistant and corrosion-resistant magnesium alloy materials are obtained.

CN118895448APending Publication Date: 2024-11-05HENAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411168630.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Magnesium alloy has poor high temperature mechanical properties, poor environmental corrosion resistance, and high production costs of high performance magnesium alloys, resulting in limited application.

Method used

By adding elements such as Al, Ca, Zn, V, Nb, Gd, etc. to improve the microstructure of the magnesium alloy, perform solid solution treatment and aging treatment, and prepare heat-resistant and corrosion-resistant magnesium alloys.

Benefits of technology

It significantly improves the high-temperature mechanical properties and corrosion resistance of magnesium alloys, reduces production costs, and obtains magnesium alloy materials with excellent comprehensive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a heat-resistant and corrosion-resistant magnesium alloy and a preparation method thereof. The heat-resistant and corrosion-resistant magnesium alloy comprises the following components in parts by mass: 1.5-2.0 parts of Al, 0.8-1.0 part of Ca, 1.2-1.6 parts of Zn, 1.3-1.5 parts of V, 1.5-2.5 parts of Nb, 2.5-3.0 parts of Gd and the balance of Mg and inevitable impurity elements. The preparation method comprises the following steps: weighing the raw materials, smelting and casting the raw materials into an as-cast alloy, and carrying out solution treatment and aging treatment on the as-cast alloy to obtain the heat-resistant and corrosion-resistant magnesium alloy. The microstructure of the magnesium alloy is improved through a multi-component alloying method, and the corrosion resistance of the alloy is remarkably improved on the basis that the high-temperature mechanical property and heat resistance of the magnesium alloy are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal alloy material preparation, and specifically relates to a heat-resistant and corrosion-resistant magnesium alloy and a preparation method thereof. Background Art

[0002] Magnesium alloys have high specific strength and specific stiffness, low density, excellent casting performance, cutting performance and high damping and vibration resistance. They have unique advantages in the existing metal structural material system and have broad application prospects. In recent years, magnesium alloys have been increasingly used as structural materials in industries such as aerospace, electronic communications and the automotive industry.

[0003] But in general, the application of magnesium alloy materials is still restricted by many factors, among which the reasons that cannot be ignored are that magnesium alloys have poor high-temperature mechanical properties, poor environmental corrosion resistance, and high production costs of high-performance magnesium alloys. Alloying is the simplest and most effective way to improve the performance of magnesium alloys. Research work on improving the mechanical properties and corrosion resistance of magnesium alloys by alloying has been widely carried out at home and abroad. Among them, adding RE, Ca, Al, Zn, Sn, Be, Si, Th, Ag, Li and other elements is more common, but it is also easy to lead to problems such as high cost of magnesium alloys and poor comprehensive performance. There are still restrictive factors in actual production.

[0004] Therefore, the exploration of magnesium alloy alloying should control the amount of expensive rare earth elements added, comprehensively and efficiently exert the beneficial effects of multi-component addition, give full play to the advantages of each component in improving the performance of magnesium alloys, and obtain magnesium alloy materials with excellent comprehensive performance. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a heat-resistant and corrosion-resistant magnesium alloy and a preparation method thereof. The present invention improves the microstructure of the magnesium alloy by a multi-component alloying method, thereby significantly improving the corrosion resistance of the alloy while improving the high-temperature mechanical properties and heat resistance of the magnesium alloy.

[0006] The present invention is achieved through the following technical solutions: The invention provides a heat-resistant and corrosion-resistant magnesium alloy, comprising the following components in parts by mass: 1.5 to 2.0 parts of Al, 0.8 to 1.0 parts of Ca, 1.2 to 1.6 parts of Zn, 1.3 to 1.5 parts of V, 1.5 to 2.5 parts of Nb, 2.5 to 3.0 parts of Gd, and the remainder being Mg and inevitable impurity elements.

[0007] Furthermore, the content of unavoidable impurity elements does not exceed 0.02 parts.

[0008] The present invention also provides a method for preparing the heat-resistant and corrosion-resistant magnesium alloy, which comprises weighing raw materials of various components and smelting and casting them into a cast alloy, and subjecting the cast alloy to solid solution treatment and aging treatment to obtain the heat-resistant and corrosion-resistant magnesium alloy.

[0009] Further, magnesium, aluminum, zinc, Mg-Ca, Mg-V, Mg-Nb, Mg-Gd master alloys are used as raw materials for smelting and casting, and the specific steps are as follows: S1. Melting raw materials magnesium, aluminum and zinc in a medium frequency induction melting furnace under gas protection; S2. When the melt temperature reaches 680-690°C, add the raw materials Mg-Ca, Mg-V, Mg-Nb, and Mg-Gd intermediate alloys, keep them warm for 5-10 minutes, then raise the temperature to 720-730°C, keep them warm for 15-20 minutes, and cast to obtain the cast alloy.

[0010] Furthermore, in S2, a steel mold is used for casting to obtain a cast alloy.

[0011] Furthermore, the solution treatment temperature is 450-470° C., and the time is 12-14 hours.

[0012] Furthermore, the aging treatment is a graded aging treatment, and the graded aging treatment is a low-temperature followed by a high-temperature aging treatment.

[0013] Furthermore, the temperature of the low-temperature aging treatment is 190-200° C., and the time of the low-temperature aging treatment is 8-10 hours; the temperature of the high-temperature aging treatment is 220-230° C., and the time of the high-temperature aging treatment is 3-4 hours.

[0014] The beneficial effects of the present invention are: (1) Aluminum is one of the commonly used alloying elements in magnesium alloys. The maximum solubility of aluminum in Mg is 12.7%. The addition of a small amount of aluminum can significantly refine the grains and improve the corrosion potential of magnesium alloys. In the present invention, the addition amount of aluminum is controlled at 1.5-2.0%. A small amount of aluminum can preferentially form compounds with vanadium and niobium elements, which can not only exert the beneficial effects of aluminum elements, but also prevent the formation of β(Mg) in the alloy. 17 Al 12 ) phase, because the β phase is an important factor that reduces the corrosion resistance and heat resistance of magnesium alloys; (2) Niobium has a very high melting point. Adding niobium to magnesium alloys can refine the microstructure and form a finely dispersed aluminum-niobium precipitate phase, optimize the distribution of the precipitate phase in the microstructure, improve the room temperature and high temperature mechanical properties of the alloy, and reduce the potential difference between the second phase and the matrix, thereby enhancing the corrosion resistance of the matrix and reducing the corrosion rate of the alloy. (3) Adding an appropriate amount of vanadium to magnesium alloys can significantly refine the structure of magnesium alloys and is an effective grain refiner. At the same time, the addition of vanadium can form fine aluminum-vanadium phases, improve the structure morphology and other phase distribution of magnesium alloys. Similarly, the addition of vanadium can increase the self-corrosion potential, stabilize the stability of the surface film, and thus improve the corrosion resistance of magnesium alloys. (4) Zinc can improve the plasticity and toughness of magnesium alloys, while increasing the allowable concentration of harmful impurities Fe, Ni, and Cu in the alloy, and improving corrosion resistance. In addition, the heat-resistant and corrosion-resistant magnesium alloy of the present invention has widely available raw materials, low alloy production costs, and a mature and stable alloy preparation process, which has a basis for mass production.

[0015] In summary, the heat-resistant and corrosion-resistant magnesium alloy of the present invention has simple components, low rare earth element content in the alloy, and low overall price. The multi-component alloying method effectively combines the improvement of the mechanical properties and corrosion resistance of the magnesium alloy. After composite alloying, the performance of the magnesium alloy is significantly improved, the room temperature and high temperature mechanical properties are significantly improved, and the corrosion resistance is also very excellent. DETAILED DESCRIPTION

[0016] The present invention provides a heat-resistant and corrosion-resistant magnesium alloy, comprising the following components in parts by mass: 1.5 to 2.0 parts of Al, 0.8 to 1.0 parts of Ca, 1.2 to 1.6 parts of Zn, 1.3 to 1.5 parts of V, 1.5 to 2.5 parts of Nb, 2.5 to 3.0 parts of Gd, and the remainder being Mg and inevitable impurity elements, wherein the content of the inevitable impurity elements does not exceed 0.02 parts.

[0017] The present invention also provides a method for preparing a heat-resistant and corrosion-resistant magnesium alloy, which uses magnesium, aluminum, zinc, Mg-Ca, Mg-V, Mg-Nb, and Mg-Gd master alloy as raw materials for smelting and casting into a cast alloy, and then subjecting the cast alloy to a solution treatment and an aging treatment to obtain a magnesium alloy. Specifically, the specific steps are: S1. Melting raw materials magnesium, aluminum and zinc in a medium frequency induction melting furnace under gas protection; When the melt temperature reaches 680-690°C, raw materials Mg-Ca, Mg-V, Mg-Nb, and Mg-Gd master alloys are added, and the temperature is kept for 5-10 minutes, and then the temperature is raised to 720-730°C, and the temperature is kept for 15-20 minutes, and a cast alloy is obtained using a steel mold; S2, performing a solution treatment, wherein the solution treatment temperature is 450-470° C. and the time is 12-14 hours; S3, perform aging treatment, the aging treatment is graded aging treatment, the graded aging treatment is low temperature followed by high temperature aging treatment. The temperature of the low temperature aging treatment is 190-200°C, and the time of the low temperature aging treatment is 8-10 hours; the temperature of the high temperature aging treatment is 220-230°C, and the time of the high temperature aging treatment is 3-4 hours.

[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below.

[0019] Embodiment 1: A heat-resistant and corrosion-resistant magnesium alloy. The components and their mass percentages of the magnesium alloy are: 1.5% Al, 1.0% Ca, 1.4% Zn, 1.4% V, 2.0% Nb, 3.0% Gd, and the balance is Mg.

[0020] Under gas protection, raw materials magnesium, aluminum and zinc are melted in a medium frequency induction melting furnace. When the melt temperature reaches 680°C, raw materials Mg-Ca, Mg-V, Mg-Nb and Mg-Gd intermediate alloys are added, and then the temperature is kept for 5 minutes, and then the temperature is raised to 720°C and kept for 18 minutes, and the alloy is cast. The cast alloy is obtained by casting using a steel mold. The solution treatment temperature is 450°C and the time is 14 hours. The aging treatment is graded aging treatment; the graded aging treatment is low temperature followed by high temperature aging treatment; the temperature of the low temperature aging treatment is 190°C and the time of the low temperature aging treatment is 10 hours; the temperature of the high temperature aging treatment is 230°C and the time of the high temperature aging treatment is 3 hours, and a heat-resistant and corrosion-resistant magnesium alloy is obtained.

[0021] Embodiment 2: A heat-resistant and corrosion-resistant magnesium alloy. The components and their mass percentages of the magnesium alloy are: 1.8% Al, 0.9% Ca, 1.6% Zn, 1.3% V, 2.5% Nb, 2.8% Gd, and the balance is Mg.

[0022] Under gas protection, raw materials magnesium, aluminum and zinc are melted in a medium frequency induction melting furnace. When the melt temperature reaches 690°C, raw materials Mg-Ca, Mg-V, Mg-Nb and Mg-Gd intermediate alloys are added, and then the temperature is kept for 8 minutes, and then the temperature is raised to 720°C, kept for 15 minutes, and the alloy is cast. The cast alloy is obtained by casting using a steel mold. The solution treatment temperature is 460°C and the time is 13 hours. The aging treatment is graded aging treatment; the graded aging treatment is low temperature followed by high temperature aging treatment; the temperature of the low temperature aging treatment is 200°C and the time of the low temperature aging treatment is 8 hours; the temperature of the high temperature aging treatment is 220°C and the time of the high temperature aging treatment is 4 hours, and a heat-resistant and corrosion-resistant magnesium alloy is obtained.

[0023] Embodiment 3: A heat-resistant and corrosion-resistant magnesium alloy. The components and their mass percentages of the magnesium alloy are: 2.0% Al, 0.8% Ca, 1.6% Zn, 1.5% V, 2.0% Nb, 2.5% Gd, and the balance is Mg.

[0024] Under gas protection, raw materials magnesium, aluminum and zinc are melted in a medium frequency induction melting furnace. When the melt temperature reaches 680°C, raw materials Mg-Ca, Mg-V, Mg-Nb and Mg-Gd intermediate alloys are added, and then the temperature is kept for 10 minutes, and then the temperature is raised to 730°C, kept for 20 minutes, and the alloy is cast. The cast alloy is obtained by casting using a steel mold. The solution treatment temperature is 470°C and the time is 12 hours. The aging treatment is graded aging treatment; the graded aging treatment is low temperature followed by high temperature aging treatment; the temperature of the low temperature aging treatment is 190°C, and the time of the low temperature aging treatment is 10 hours; the temperature of the high temperature aging treatment is 230°C, and the time of the high temperature aging treatment is 3 hours, and a heat-resistant and corrosion-resistant magnesium alloy is obtained.

[0025] Embodiment 4: A heat-resistant and corrosion-resistant magnesium alloy. The components and their mass percentages of the magnesium alloy are: 2.0% Al, 1.0% Ca, 1.2% Zn, 1.3% V, 1.5% Nb, 3.0% Gd, and the balance is Mg.

[0026] Under gas protection, raw materials magnesium, aluminum and zinc are melted in a medium frequency induction melting furnace. When the melt temperature reaches 690°C, raw materials Mg-Ca, Mg-V, Mg-Nb and Mg-Gd intermediate alloys are added, and then the temperature is kept for 10 minutes, and then the temperature is raised to 730°C, kept for 20 minutes, and the alloy is cast. The cast alloy is obtained by casting using a steel mold. The solution treatment temperature is 460°C and the time is 14 hours. The aging treatment is graded aging treatment; the graded aging treatment is low temperature followed by high temperature aging treatment; the temperature of the low temperature aging treatment is 200°C, and the time of the low temperature aging treatment is 8 hours; the temperature of the high temperature aging treatment is 220°C, and the time of the high temperature aging treatment is 4 hours, and a heat-resistant and corrosion-resistant magnesium alloy is obtained.

[0027] The raw materials involved in the specific implementation of the present invention are all commercially available products. Mechanical properties tests and corrosion test tests were carried out on Examples 1 to 4. The mechanical properties tests were carried out in accordance with the national standard GB6397-86 "Metal Tensile Test Specimen". The corrosion test was measured according to the immersion weight loss method. The corrosive liquid was 3.5% NaCl solution and the immersion time was 24 hours. The specific experimental results are shown in Tables 1 and 2 below; Table 1 Room temperature and high temperature tensile mechanical properties of heat-resistant and corrosion-resistant magnesium alloys in Examples 1 to 4 It can be seen from Table 1 that the room temperature tensile strength of the heat-resistant and corrosion-resistant magnesium alloy obtained by the present invention reaches 259-273MPa, the yield strength is 158-182MPa, and the elongation is 4.9-6.1%; while the tensile strength at 225°C is 209-221MPa, the yield strength is 127-136MPa, and the elongation is 8.9-10.5%. The above results show that the alloy not only has excellent room temperature mechanical properties, but also has a small reduction in high temperature mechanical properties.

[0028] Table 2 Corrosion rate of heat-resistant and corrosion-resistant magnesium alloys in Examples 1 to 4 It can be directly concluded from Table 2 that the corrosion rate of the corrosion sample obtained by the embodiment of the present invention is only 0.147~0.187mg·cm -2 ·d -1 , the corrosion resistance is very excellent.

[0029] In summary, the heat-resistant and corrosion-resistant magnesium alloy of the present invention meets the requirements of the environment on high-temperature mechanical properties and corrosion resistance on the basis of controlling the amount of rare earth addition.

[0030] It should be noted that although the present invention is described by the above embodiments, the present invention may also have other various embodiments. Without departing from the spirit and scope of the present invention, it is obvious that those skilled in the art may make various corresponding changes and deformations to the present invention, but these changes and deformations should all fall within the scope of protection of the appended claims of the present invention and their equivalents.

Claims

1. A heat-resistant and corrosion-resistant magnesium alloy, characterized in that: The invention comprises the following components in parts by mass: 1.5 to 2.0 parts of Al, 0.8 to 1.0 parts of Ca, 1.2 to 1.6 parts of Zn, 1.3 to 1.5 parts of V, 1.5 to 2.5 parts of Nb, 2.5 to 3.0 parts of Gd, and the balance is Mg and unavoidable impurity elements.

2. The heat-resistant and corrosion-resistant magnesium alloy according to claim 1, characterized in that: The content of unavoidable impurity elements shall not exceed 0.02 parts.

3. The method for preparing a heat-resistant and corrosion-resistant magnesium alloy according to any one of claims 1 to 2, characterized in that: The raw materials of various components are weighed and melted and cast into a cast alloy, and the cast alloy is subjected to a solid solution treatment and an aging treatment to obtain a heat-resistant and corrosion-resistant magnesium alloy.

4. The method for preparing a heat-resistant and corrosion-resistant magnesium alloy according to claim 3, characterized in that: Using magnesium, aluminum, zinc, Mg-Ca, Mg-V, Mg-Nb, Mg-Gd master alloy as raw materials for smelting and casting, the specific steps are as follows: S1. Melting raw materials magnesium, aluminum and zinc in a medium frequency induction melting furnace under gas protection; S2. When the melt temperature reaches 680-690°C, add the raw materials Mg-Ca, Mg-V, Mg-Nb, and Mg-Gd intermediate alloys, keep them warm for 5-10 minutes, then raise the temperature to 720-730°C, keep them warm for 15-20 minutes, and cast to obtain the cast alloy.

5. The method for preparing a heat-resistant and corrosion-resistant magnesium alloy according to claim 4, characterized in that: In S2, a steel mold is used for casting to obtain a cast alloy.

6. The method for preparing a heat-resistant and corrosion-resistant magnesium alloy according to claim 3, characterized in that: The solution treatment temperature is 450-470° C. and the time is 12-14 hours.

7. The method for preparing a heat-resistant and corrosion-resistant magnesium alloy according to claim 3, characterized in that: The aging treatment is a graded aging treatment, and the graded aging treatment is a low-temperature followed by a high-temperature aging treatment.

8. The method for preparing a heat-resistant and corrosion-resistant magnesium alloy according to claim 7, characterized in that: The temperature of the low-temperature aging treatment is 190-200° C., and the time of the low-temperature aging treatment is 8-10 hours; the temperature of the high-temperature aging treatment is 220-230° C., and the time of the high-temperature aging treatment is 3-4 hours.