Preparation method of modified maleimide resin as well as resin composition and application of modified maleimide resin
A modified maleimide resin composition, prepared via prepolymerization with alicyclic and aliphatic diamines, addresses the limitations of bismaleimide resins, providing improved heat resistance, toughness, and dielectric properties for high-density circuit boards.
Patent Information
- Application Number
- CN202411321327.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
Existing bismaleimide resins used in copper clad laminates face issues such as high curing temperature, large water absorption, brittleness, and limited improvements in toughness, heat resistance, and dielectricity, which hinder their performance in high-density, high-speed signal transmission applications.
A prepolymerization process involving maleimide resin with alicyclic diamine and aliphatic diamine compounds, along with aminophenol, to create a modified maleimide resin with improved heat resistance, toughness, low thermal expansion coefficient, and reduced dielectricity, using specific organic solvents and catalysts to enhance compatibility and flexibility.
The modified resin composition achieves high heat resistance, toughness, low dielectric constant, and low water absorption, enhancing the performance of copper clad laminates for high-density circuit boards.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper clad laminates, and in particular to a preparation method of a modified maleimide resin, a resin composition and applications thereof. Background Art
[0002] In recent years, as electronic signal transmission methods develop towards 5G, and electronic equipment, communication devices, personal computers, etc. are becoming more functional and miniaturized, the circuit boards used are also developing towards multi-layering, high-density wiring, and high-speed signal transmission, which puts higher requirements on the comprehensive performance of circuit substrates such as copper clad laminates. In order to avoid deformation of copper clad laminates caused by the use of high-temperature processes during product processing, which in turn causes defects in subsequent products and causes abnormal signal transmission, it is necessary to develop copper clad laminate materials with a lower thermal expansion coefficient.
[0003] Bismaleimide resin has excellent heat resistance, high modulus, low CTE, and is therefore widely used in high performance printed circuit boards. However, there are problems such as high curing temperature, large water absorption, large brittleness in bismaleimide resin. In order to improve the above-mentioned shortcomings of maleimide resin, diamine or allyl compound modification is generally used at present, wherein, the product after modified bismaleimide with aromatic diamine compounds is all improved to a certain extent in solubility and toughness, but the aromatic diamine toxicity is larger, and the modified product can only be dissolved in high boiling point polar solvents (such as DMF, NMP etc.), and it still has a large improvement space in toughness, heat resistance, dielectricity and water absorption.
[0004] Therefore, in view of the above problems, the present invention proposes a preparation method of a modified maleimide resin and a resin composition and application thereof to obtain a resin composition with high heat resistance, high toughness, low CTE, low dielectricity and low water absorption. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method of a modified maleimide resin and a resin composition and application thereof, so as to obtain a resin composition with high heat resistance, high toughness, low CTE, low dielectricity and low water absorption.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The preparation method of the modified maleimide resin comprises the following steps: prepolymerizing 100 parts of maleimide resin and 1 to 130 parts of alicyclic diamine by weight;
[0008] The alicyclic diamine is represented by the structural formula (1):
[0009]
[0010] Wherein, X is a C6-C30 alicyclic group, R1, R2, R3 and R4 are the same or different, and are hydrogen or a C1-C5 alkyl group respectively.
[0011] Preferably, the X group in the structural formula (1) is One or more structures in .
[0012] Preferably, the prepolymerization reaction temperature is 60 to 200° C., and the reaction time is 0.5 to 5 hours.
[0013] Preferably, 5 to 40 parts of aliphatic diamine compound are added during the prepolymerization process.
[0014] Preferably, the aliphatic diamine compound is any diamine compound containing a C2-C36 alkylene group in its molecular structure.
[0015] More preferably, the aliphatic diamine compound is selected from one or more of dimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine and decamethylenediamine.
[0016] When an appropriate amount of aliphatic diamine compounds is added during the prepolymerization process, the flexibility is further increased in the polyphenyl ring cross-linked network structure, the warping of the cured product is improved, and at the same time, the heat resistance, dielectric properties and water absorption are improved on the basis of satisfying good compatibility and controlling costs; this structure increases the distance between molecular layers, creates more free space volume, makes it easier for the molecular layers to slide, and thus achieves a toughening effect.
[0017] The method of the prepolymerization reaction is not particularly limited. The amine compound and the maleimide resin are dissolved and dispersed in an appropriate amount of an organic solvent, heated to 60-200° C. under nitrogen protection and reacted for 0.5-5 hours under stirring conditions to obtain a modified bismaleimide prepolymer.
[0018] Preferably, the organic solvent is selected from at least one of acetone, butanone, toluene, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene and cyclohexane.
[0019] Aminophenol compounds are added during the prepolymerization of maleimide resin and amine compounds to control the overall reaction rate, improve processability, and improve the comprehensive properties of the cured product.
[0020] Preferably, the amount of aminophenol added is 0.5 to 5 parts based on 100 parts of the total amount of the maleimide resin and the amine compound.
[0021] The aminophenol is preferably 4-aminophenol.
[0022] The prepolymerization method comprises dissolving and dispersing an amine compound, a maleimide resin and an aminophenol in an appropriate amount of an organic solvent, heating to 60 to 180° C. under nitrogen protection and reacting for 0.5 to 5 hours under stirring conditions to obtain an amine-modified bismaleimide prepolymer.
[0023] The present application also claims protection for a resin composition, which comprises, by weight, the above-mentioned modified maleimide resin.
[0024] Preferably, the resin composition comprises, by weight:
[0025] Modified maleimide resin: 50-100 parts;
[0026] Inorganic filler: 10-200 parts;
[0027] Preferably, the resin composition further comprises at least one of epoxy resin, cyanate resin, polyphenylene ether resin, benzoxazine resin, hydrocarbon resin or phenolic resin.
[0028] In the above technical scheme, the cyanate ester compound is selected from at least one of bisphenol A type cyanate ester compounds, bisphenol F type cyanate ester compounds, bisphenol E type cyanate ester compounds, bisphenol M type cyanate ester compounds, DCPD type cyanate ester compounds, naphthalene type cyanate ester compounds, biphenyl type cyanate ester compounds, and triphenyl type cyanate ester compounds.
[0029] The cyanate compound is a monomer, a prepolymer or a mixture thereof.
[0030] In the above technical scheme, the epoxy resin is selected from one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol E epoxy resin, phosphorus-containing epoxy resin, o-cresol epoxy resin, bisphenol A novolac epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, triphenylmethane epoxy resin, tetraphenylethane epoxy resin, biphenyl epoxy resin, naphthalene ring epoxy resin, dicyclopentadiene epoxy resin, isocyanate epoxy resin, aralkyl linear phenolic epoxy resin, alicyclic epoxy resin, glycidyl amine epoxy resin, glycidyl ether epoxy resin, and glycidyl ester epoxy resin.
[0031] In the above technical solution, the polyphenylene ether resin is represented by structural formula (13):
[0032]
[0033] Among them, X is or / and R 11 , R 12 , R 13 , R 14 , R15 , R 16 , R 17 and R 18 are hydrogen or C1-C5 alkyl, B is C1-C20 alkylene or oxy; Y is R 21 , R 22 , R 23 and R 24 are hydrogen or C1-C5 alkyl.
[0034] Specifically, the polyphenylene ether resin is selected from OPE-2ST series products manufactured by Mitsubishi Gas.
[0035] In the above technical solution, the benzoxazine resin is selected from one or a combination of at least two of bisphenol A type benzoxazine resin, dicyclopentadiene type benzoxazine resin, bisphenol F type benzoxazine resin, phenolphthalein type benzoxazine resin, MDA type benzoxazine resin, ODA type benzoxazine resin or unsaturated bond-terminated benzoxazine resin.
[0036] In the above technical solution, the hydrocarbon resin contains 1,2-vinyl, and the 1,2-vinyl content is ≥70%. Preferably, the 1,2-vinyl content in the hydrocarbon resin is 80-98%.
[0037] Preferably, the inorganic filler is selected from at least one of fused silica, crystalline silica, spherical silica, hollow silica, aluminum hydroxide, aluminum oxide, talc, aluminum nitride, boron nitride, silicon carbide, barium sulfate, barium titanate, strontium titanate, calcium carbonate, calcium silicate, mica, and glass fiber powder.
[0038] More preferably, the inorganic filler is silicon dioxide.
[0039] More preferably, the inorganic filler is surface-treated spherical silica.
[0040] The surface treatment agent is a silane coupling agent, such as a silane coupling agent containing an epoxy group, an amino group, a vinyl group, an acrylate group or an allyl group.
[0041] Preferably, the median particle size of the inorganic filler is 1 to 15 microns, for example, 1 micron, 2 microns, 5 microns, 8 microns, 10 microns, 11 microns, 12 microns, 13 microns, 14 microns.
[0042] More preferably, the median particle size of the inorganic filler is 1 to 10 microns.
[0043] In the above technical solution, the resin composition also includes a catalyst, and its content is 0.01 to 8 parts by weight.
[0044] The catalyst is selected from at least one of imidazoles, pyridines, organic phosphorus and metal salts.
[0045] Preferably, the imidazole is selected from at least one of 4-dimethylaminopyridine, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, modified imidazole and zinc octanoate.
[0046] In the above technical solution, the resin composition also includes a flame retardant, which contains 5 to 60 parts by weight.
[0047] The flame retardant is selected from at least one of a bromine flame retardant, a phosphorus flame retardant, a nitrogen flame retardant, an organic silicon flame retardant, and an organic metal salt flame retardant.
[0048] Preferably, the brominated flame retardant is selected from at least one of decabromodiphenyl ether, decabromodiphenyl ethane, brominated styrene or tetrabromophthalamide;
[0049] The phosphorus flame retardant is selected from inorganic phosphorus, condensed phosphate, phosphoric acid, hypophosphite, phosphorus oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ), (m is an integer from 1 to 5), At least one of 10-phenyl-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tris(2,6-dimethylphenyl)phosphine, phosphazene, and modified phosphazene, wherein the DOPO group in the above structure is
[0050] Preferably, the flame retardant is a condensed phosphate ester, a hypophosphite or a bis-DOPO compound.
[0051] The present application also claims to protect the application of a resin composition, which is the application of the above-mentioned resin composition in prepregs, laminates, insulating films, insulating boards, copper-clad boards, circuit substrates and electronic devices.
[0052] Specifically, the prepreg comprises a reinforcing material and the above-mentioned resin composition attached to the surface of the reinforcing material.
[0053] Preferably, the preparation method of the prepreg is:
[0054] Dissolving the resin composition with a solvent to prepare a resin composition glue solution;
[0055] The reinforcing material is immersed in the resin composition glue solution, and the immersed reinforcing material is taken out and baked at a temperature of 100 to 180° C. for 1 to 15 minutes, and the semi-cured sheet can be obtained after drying.
[0056] Preferably, the solvent is selected from at least one of acetone, butanone, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene and cyclohexane.
[0057] Preferably, the reinforcing material is selected from at least one of natural fibers, organic synthetic fibers, organic fabrics, and inorganic fabrics. Preferably, the reinforcing material is glass fiber cloth, and the glass fiber cloth is preferably open fiber cloth or flat cloth. More preferably, the glass fiber cloth is E glass fiber cloth, S glass fiber cloth, T glass fiber cloth or Q glass fiber cloth.
[0058] In addition, when the reinforcing material is glass fiber cloth, the glass fiber cloth generally needs to be chemically treated to improve the bonding between the resin composition and the interface of the glass fiber cloth. The main method of the chemical treatment is coupling agent treatment. The coupling agent used is preferably an epoxy silane coupling agent or an amino silane coupling agent, so that the reinforcing material has good water resistance and heat resistance.
[0059] Preferably, the laminate comprises a piece of the above-mentioned prepreg and a metal foil arranged on at least one side of the prepreg, or the laminate comprises a composite sheet formed by overlapping a plurality of the above-mentioned prepregs and a metal foil arranged on at least one side of the composite sheet.
[0060] Preferably, the method for preparing the laminate is:
[0061] The laminated board can be obtained by coating one or both sides of the prepreg with metal foil, or by stacking at least two prepregs to form a composite sheet, coating one or both sides of the composite sheet with metal foil, and hot pressing.
[0062] The hot pressing conditions are: pressing for 2 to 4 hours at a pressure of 0.2 to 2 MPa and a temperature of 150 to 250°C.
[0063] Preferably, the metal foil is selected from copper foil or aluminum foil, and the thickness of the metal foil is not particularly limited, such as 5 μm, 8 μm, 12 μm, 18 μm, 35 μm or 70 μm.
[0064] Preferably, the insulating plate includes at least one prepreg sheet mentioned above.
[0065] Preferably, the insulating film comprises a carrier film and the above-mentioned resin composition attached to the surface of the carrier film, and the heat resistance of the insulating film is significantly improved.
[0066] Preferably, the method for preparing the insulating film is:
[0067] Dissolving the resin composition with a solvent to prepare a resin composition glue solution;
[0068] The insulating film can be obtained by coating the resin composition glue on the carrier film and heating and drying the carrier film coated with the resin composition glue.
[0069] Preferably, the solvent is selected from at least one of acetone, butanone, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene and cyclohexane.
[0070] Preferably, the carrier film is selected from at least one of PET film, PP film, PE film and PVC film.
[0071] Preferably, the circuit substrate includes at least one of the prepreg and the laminate.
[0072] Preferably, the method for preparing the circuit substrate is a conventional technical means in the art and will not be described in detail here.
[0073] Preferably, the electronic device comprises the above-mentioned circuit substrate.
[0074] Preferably, the method for preparing the electronic device is a conventional technical means in the art and will not be described in detail here.
[0075] Due to the application of the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0076] 1. The present invention uses an aromatic amine compound containing multiple alicyclic structures or heterocyclic structures to modify the maleimide resin, wherein the structure is a special spatial structure, which makes the obtained material have high stability and reactivity, and is conducive to prepolymerization with bismaleimide;
[0077] 2. The present invention comprises a plurality of homogeneous or heterocyclic structures to form an alicyclic group, so that the prepolymer has better dielectric properties, and obtains a higher glass transition temperature and heat resistance. The diamine of the alicyclic structure has a large free volume, can break the crystallinity of the BMI monomer, expand the distance between the molecular chains, and improve the solubility of the resin prepreg in common solvents. The alicyclic ring has extremely low polarity, which greatly improves the dielectric properties of BMI. In addition, the amino group and the ether bond in the structure are in the para or meta position, so that the flexibility is increased, and the adhesion between layers and between layers and metals is improved, so as to obtain a cured product with high heat resistance, high toughness, low CTE, low dielectric properties, and low water absorption, thereby obtaining a cured product with relatively excellent comprehensive performance, which is conducive to its large-scale application. DETAILED DESCRIPTION
[0078] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, a specific implementation scheme is now described in detail.
[0079] The present invention is further described below in conjunction with the examples, but the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not indicated are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.
[0080] Synthesis Example 1: Prepolymer A;
[0081] Add 50g of 100 g of maleimide resin (BMI-2300, manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were reacted at 160° C. for 100 min to obtain prepolymer A.
[0082] Synthesis Example 2: Prepolymer B;
[0083] Add 50g of 100 g of maleimide resin (BMI-2300, manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were reacted at 160° C. for 100 min to obtain prepolymer B.
[0084] Synthesis Example 3: Prepolymer C;
[0085] Add 30g of 20 g of hexamethylenediamine, 100 g of maleimide resin (MIR-3000, manufactured by Nippon Kayaku Co., Ltd.), and 2.5 g of p-aminophenol were reacted at 130° C. for 100 min to obtain prepolymer C.
[0086] Compared with Synthesis Example 1, Synthesis Example 3 adds an aliphatic diamine compound other than the structural formula (1).
[0087] Synthesis Example 4: Prepolymer D;
[0088] Add 100g of maleimide resin (BMI-2300 manufactured by Yamato Chemical Industry Co., Ltd.) and 2g of p-aminophenol to a beaker, react at 110°C for 60min, then heat to 150°C and add 55g of The reaction was continued for 60 min to obtain prepolymer D.
[0089] Comparative Synthesis Example 1: Prepolymer E;
[0090] 40 g of 4,4'-diaminodiphenylmethane, 100 g of maleimide resin (BMI-2300 manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were added to a beaker and reacted at 120°C for 100 min to obtain a prepolymer E.
[0091] The amine compound used in Comparative Synthesis Example 1 is different from that in Synthesis Example 1, and the amine compound in Comparative Synthesis Example 1 does not contain an ether bond.
[0092] Comparative Synthesis Example 2: Prepolymer F;
[0093] 40 g of 4,4'-diaminodiphenyl ether, 100 g of maleimide resin (BMI-2300 manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were added to a beaker and reacted at 120°C for 100 min to obtain a prepolymer F.
[0094] The ether bond-containing aromatic amine compound used in Comparative Synthesis Example 2 is different from that in Synthesis Example 1. The aromatic amine compound in Comparative Synthesis Example 2 contains only one ether bond.
[0095] Example 1
[0096] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer A, 30 parts of cyanate ester, 20 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0097] Example 2
[0098] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer B, 20 parts of cyanate ester, 30 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0099] Example 3
[0100] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer C, 15 parts of cyanate ester, 10 parts of epoxy resin, 125 parts of inorganic filler, and 0.5 parts of catalyst.
[0101] Example 4
[0102] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer D, 60 parts of polyphenylene ether resin, 20 parts of cross-linking agent, 180 parts of inorganic filler, and 0.5 parts of catalyst.
[0103] Comparative Example 1
[0104] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer E, 30 parts of cyanate ester, 20 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0105] Comparative Example 2
[0106] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer F, 20 parts of cyanate ester, 30 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0107] Comparative Example 3
[0108] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer F, 60 parts of polyphenylene ether resin, 20 parts of cross-linking agent, 180 parts of inorganic filler, and 0.5 parts of catalyst.
[0109] The components and addition amounts of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1 below.
[0110] Table 1
[0111] Components Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Prepolymer A 100 Prepolymer B 100 Prepolymer C 100 Prepolymer D 100 Prepolymer E 100 Prepolymer F 100 100 Cyanate 30 20 15 30 20 Epoxy resin 20 30 10 20 30 Polyphenylene ether resin 60 60 Crosslinking agent 20 20 Inorganic fillers 150 150 125 180 150 150 180 catalyst 0.5 0.5 0.5 0.5 0.5 0.5 0.5
[0112] The raw material manufacturers and brands of each component used in Examples 1-4 and Comparative Examples 1-3 are shown in Table 2 below.
[0113] Table 2
[0114] Components Manufacturer and brand Cyanate Made by Tianqi, bisphenol A Epoxy resin DIC, HP-6000 Polyphenylene ether resin Made by Mitsubishi, OPE-2St Crosslinking agent TAIC Inorganic fillers Silicon dioxide catalyst 2-Methylimidazole
[0115] Mixing of glue:
[0116] According to the formula in Table 1, all the components in the formula are prepared into a thermosetting resin composition glue solution with a solid content of 65%;
[0117] Then a laminate was made under the following conditions:
[0118] Reinforcement material: ordinary electronic grade 2116 glass fiber cloth;
[0119] Metal foil: 18 microns, electrolytic copper foil;
[0120] Number of layers: 6;
[0121] Thickness of sheet after forming: 0.7mm;
[0122] Pre-impregnation semi-curing conditions: 170℃ / 5min;
[0123] Curing conditions: 150℃ / 60min+220℃ / 180min;
[0124] The performance tests were carried out on the above-mentioned embodiments 1-4 and comparative examples 1-3 respectively, and the test results are shown in Table 3 below.
[0125] Table 3
[0126] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Glass transition temperature (DMA / ℃) 251 252 249 245 234 237 226 PCT water absorption % 0.29 0.31 0.26 0.21 0.45 0.48 0.45 CTE (X / Y axis) (ppm / ℃) 5.0 5.3 5.4 5.5 11.0 9.9 11.1 Peel strength (N / mm) 1.0 0.97 1.12 0.88 1.1 0.96 0.89 Dielectric constant (10GHz) 3.35 3.31 3.37 3.12 3.79 3.67 3.34 Dielectric loss (10GHz) 0.0035 0.0033 0.0037 0.0028 0.0071 0.0065 0.0030 Elastic modulus(GPa) 29 29 32 33 23 25 24
[0127] The performance of the above-mentioned Examples 1-4 and Comparative Examples 1-3 was tested as follows:
[0128] (1) Glass transition temperature (Tg): dynamic mechanical properties tester (TADMAQ800, USA) was used with a heating rate of 10 °C / min and a nitrogen atmosphere;
[0129] (2) Dk and Df: measured at 10 GHz using the flat plate method in accordance with IPC-TM-6502.5.5.9;
[0130] (3) CTE (X / Y) determination: TMA (thermomechanical analysis) was used, with a heating rate of 10°C / min and a test temperature range of 30 to 100°C;
[0131] (4) PCT water absorption rate: Take 3 samples of 10 cm × 10 cm, 0.80 mm thick, with metal foil removed from both sides, dry them at 120°C for 2 hours, weigh them, and record the weight as W1. Then use a pressure cooker tester to treat them at 121°C and 2 atmospheres for 12 hours. After absorbing the free water on the surface, put them in a desiccator and cool them down. Then weigh them as W2. The water absorption rate of the board is calculated based on the weight before and after.
[0132] (5) Peel strength (PS): The peel strength of the metal cover layer was tested using a laminate according to the “after thermal stress” test conditions in the IPC-TM-650 method.
[0133] (6) Elastic modulus: measured according to the DMA method specified in IPC-TM-6502.4.24.4;
[0134] (7) Appearance quality: Visually inspect the appearance of the CCL substrate. A substrate without obvious glue deficiency or pinholes has a good appearance. A substrate with glue deficiency or pinholes has a fair appearance.
[0135] In summary, the present invention uses an aromatic amine compound containing multiple alicyclic structures or heterocyclic structures to modify the maleimide resin, wherein the structure is a special spatial structure form, which makes the obtained material have high stability and reactivity, and is conducive to prepolymerization with bismaleimide; the alicyclic group is composed of multiple homogeneous or heterocyclic structures, so that the prepolymer has better dielectric properties, and obtains higher glass transition temperature and heat resistance. The diamine of this alicyclic structure has a large free volume, which can break the crystallinity of the BMI monomer, expand the distance between molecular chains, and improve the solubility of the resin prepreg in common solvents. The alicyclic ring has extremely low polarity, which greatly improves the dielectric properties of BMI; in addition, the amino group and the ether bond in the structure are in the para position or meta position, so that the flexibility is increased, the adhesion between layers and between layers and metals is improved, and a cured product with high heat resistance, high toughness, low CTE, low dielectric properties, and low water absorption is obtained, thereby obtaining a cured product with relatively excellent comprehensive performance, which is conducive to its large-scale application.
[0136] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a modified maleimide resin, characterized in that: By weight, 100 parts of maleimide resin and 1 to 130 parts of alicyclic diamine are prepolymerized to form; The alicyclic diamine is represented by the structural formula (1): Wherein, X is a C6-C30 alicyclic group, R1, R2, R3 and R4 are the same or different, and are hydrogen or a C1-C5 alkyl group respectively.
2. The method for preparing the modified maleimide resin according to claim 1, characterized in that: The X group in the structural formula (1) is One or more structures in .
3. The method for preparing the modified maleimide resin according to claim 1, characterized in that: The temperature of the prepolymerization reaction is 60-200° C., and the reaction time is 0.5-5 hours.
4. The method for preparing the modified maleimide resin according to claim 1, characterized in that: In parts by weight, 5 to 40 parts of aliphatic diamine compound are added during the prepolymerization reaction.
5. The method for preparing the modified maleimide resin according to claim 4, characterized in that: The aliphatic diamine compound is any diamine compound containing a C2-C36 alkylene group in its molecular structure.
6. A resin composition, characterized in that In parts by weight, it comprises: the modified maleimide resin according to any one of claims 1 to 5.
7. The resin composition according to claim 6, characterized in that The resin composition comprises, by weight: Modified maleimide resin: 50-100 parts; Inorganic filler: 10 to 200 parts.
8. The resin composition according to claim 7, characterized in that The resin composition further comprises at least one of epoxy resin, cyanate resin, polyphenylene ether resin, benzoxazine resin, hydrocarbon resin or phenolic resin.
9. The resin composition according to claim 7, characterized in that The inorganic filler is selected from at least one of fused silica, crystalline silica, spherical silica, hollow silica, aluminum hydroxide, aluminum oxide, talc, aluminum nitride, boron nitride, silicon carbide, barium sulfate, barium titanate, strontium titanate, calcium carbonate, calcium silicate, mica, and glass fiber powder.
10. Use of the resin composition according to any one of claims 6 to 9 in prepregs, laminates, insulating films, insulating boards, copper-clad boards, circuit substrates and electronic devices.