Copper-based catalyst as well as preparation method and application thereof

Through the cerium doping and electrochemical oxidation-immersion-heat treatment methods of copper-based catalysts, the problems of selectivity and low efficiency of existing copper-based catalysts are solved, and efficient catalytic carbon dioxide reduction is achieved to prepare ethylene, which improves Faraday efficiency and yield. Suitable for large-scale applications.

CN118895523APending Publication Date: 2024-11-05UNIV OF MACAU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185483.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing copper-based catalysts have problems of low selectivity and low catalytic efficiency when preparing ethylene by catalyzing carbon dioxide reduction, resulting in the Faraday efficiency generally being less than 40%, and the resulting products are diverse, making it difficult to achieve large-scale commercial application.

Method used

The copper-based catalyst is prepared from cerium-doped copper oxide on the copper substrate and the substrate surface. The layered structure is formed by electrochemical oxidation method, and the cerium ions are uniformly doped with immersion method to form a high specific surface area, excellent selectivity and catalytic activity. catalyst.

Benefits of technology

It improves the selectivity and stability of the catalyst, improves the Faraday efficiency and yield of ethylene prepared by carbon dioxide reduction, and is suitable for the large-scale application of electrochemical carbon dioxide reduction, realizing the resource utilization of carbon dioxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895523A_ABST
    Figure CN118895523A_ABST
Patent Text Reader

Abstract

The invention discloses a copper-based catalyst as well as a preparation method and application thereof, and relates to the technical field of catalysts. The catalyst comprises a substrate and cerium-doped copper oxide on the surface of the substrate, the substrate comprises copper; the mass content of cerium in the cerium-doped copper oxide is 1-6%. The copper-based catalyst with high Faraday efficiency for preparing ethylene by reducing carbon dioxide is prepared by taking a copper sheet as a substrate and adopting a simple electrochemical oxidation-soaking-heat treatment composite method, the ethylene yield is high, the selectivity and the stability are relatively high, and the copper-based catalyst is suitable for large-scale application of electrochemical carbon dioxide reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalytic technology, and in particular to a copper-based catalyst and a preparation method and application thereof. Background Art

[0002] With the development of society, energy consumption is increasing. While burning fossil energy to obtain the power consumption required to maintain society, it also brings a series of environmental problems. Among them, the large amount of carbon dioxide produced by combustion is the main cause of global warming, sea level rise, sea acidification and marine ecosystem collapse. In order to solve the environmental and energy problems caused by excessive carbon dioxide emissions, in addition to utilizing renewable green energy such as solar energy, wind energy, tidal energy, etc., utilizing the emitted carbon dioxide is also one of the solutions. A series of carbon-containing molecules produced by carbon dioxide reduction are important fuels and chemical raw materials. Therefore, converting emitted carbon dioxide into valuable carbon-containing molecules is a solution that can not only reduce the amount of carbon dioxide in the atmosphere, alleviate the environmental crisis, achieve "carbon neutrality", but also produce useful fuels and chemical raw materials.

[0003] Ethylene is an important chemical raw material and can also be used as a precursor for the synthesis of liquid fuels. It also has the advantage of high energy density and can be used as a good energy storage carrier to achieve the conversion and storage of green energy based on carbon dioxide. At present, the catalyst used for the reduction of carbon dioxide to produce ethylene is mainly copper. Copper is environmentally friendly, abundant in resources, and has an easily adjustable structure. It is a promising catalyst material for the reduction of carbon dioxide to ethylene. However, the current copper-based catalyst catalyzed carbon dioxide reduction of ethylene still has the following defects and cannot be used on a large scale commercially: (1) Low catalytic selectivity: The decomposition of water may cause serious hydrogen evolution reaction, reducing the Faraday efficiency of carbon dioxide reduction to ethylene, resulting in a very diverse final product obtained during the carbon dioxide reduction process. In addition to ethylene, it also includes carbon monoxide (CO), methane (CH4), methanol (CH3OH), formic acid (HCOOH), ethanol (C2H5OH), ethane (C2H6) and n-propanol (C3H7OH). At present, the Faraday efficiency of copper-based catalysts to produce ethylene is generally less than 40%, generally between 10 and 30%; (2) Low catalytic efficiency: Carbon dioxide has stable chemical properties, and the production of ethylene requires high energy barrier CC coupling, which requires a high overpotential and makes the yield of ethylene low. Therefore, the development of non-precious metal catalysts with high activity, high selectivity and high stability, as well as low price, high efficiency and long life for the reduction of carbon dioxide to produce ethylene is crucial to the development of the commercial electrochemical reduction of carbon dioxide to produce ethylene industry. Summary of the invention

[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the purpose of the present invention is to provide a copper-based catalyst with high specific surface area, excellent selectivity and catalytic activity, good stability, low price, high efficiency and long life.

[0005] A second aspect of the present invention provides a method for preparing a copper-based catalyst.

[0006] The third aspect of the present invention provides a use of a copper-based catalyst.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] The first aspect of the present invention provides a copper-based catalyst, comprising a substrate and cerium-doped copper oxide on the surface of the substrate; the substrate comprises copper; the mass content of cerium in the cerium-doped copper oxide is 1-6%.

[0009] The copper-based catalyst of the present invention has high specific surface area, excellent selectivity and catalytic activity, good stability, low price, high efficiency and long life, and can be used for high-efficiency catalytic reduction of carbon dioxide to prepare ethylene.

[0010] In some embodiments of the present invention, the mass content of cerium in the cerium-doped copper oxide is 2-5%.

[0011] In some embodiments of the present invention, the mass content of cerium in the cerium-doped copper oxide is 3-4%.

[0012] In some embodiments of the present invention, the thickness of the cerium-doped copper oxide on the surface of the substrate is 1 to 3 μm.

[0013] In some embodiments of the present invention, the thickness of the cerium-doped copper oxide on the surface of the substrate is 1.5-2.5 μm.

[0014] The second aspect of the present invention provides a method for preparing the copper-based catalyst according to the first aspect of the present invention, comprising the following steps:

[0015] The copper sheet is used as the anode and immersed in the electrolyte together with the cathode for electrochemical oxidation;

[0016] Soaking the electrochemically oxidized copper sheet in a soluble cerium salt solution to obtain a catalyst precursor;

[0017] The catalyst precursor is heat-treated to obtain the copper-based catalyst.

[0018] The present invention adopts an electrochemical oxidation method, which has the following advantages: electrochemical oxidation of copper sheets to prepare copper oxide, forming basic copper carbonate in the electrolyte. Basic copper carbonate has a layered structure, and the interlayers can generate an electrostatic interaction mode with cerium ions, adsorb cerium ions, and ensure uniform cerium doping.

[0019] At the same time, compared with the direct mixing of cerium salt powder and electrochemically oxidized copper sheet for annealing, the present invention immerses the electrochemically oxidized copper sheet in a soluble cerium salt solution. This immersion method has the following advantages: (1) The method is simple and the doping is uniform: the mixing method requires the use of mixing equipment, such as a ball mill, to achieve the purpose of uniform mixing, while the present invention uses the immersion method to directly prepare uniformly cerium-doped materials on a large-area copper sheet substrate; (2) Self-supporting large-area electrode materials can be prepared: the mixing method can only prepare powdered samples, which still need to be further coated with a conductive substrate and formed to obtain a catalyst, while the present invention uses the immersion method without complicated grinding and forming processes, and only two simple steps of immersion and annealing are required to obtain a large-area catalyst.

[0020] It should be noted that, since a hydroxide protective layer has been formed on the surface of the copper sheet during the electrochemical oxidation and immersion in the cerium salt solution, the inside of the copper sheet will not oxidize during the heat treatment process, while the cerium-doped basic copper carbonate on the surface forms cerium-doped copper oxide.

[0021] In some embodiments of the present invention, the preparation method does not include the steps of coating, grinding, ball milling, and molding.

[0022] In some embodiments of the present invention, the concentration of the soluble cerium salt solution is 2 to 20 mmol / L.

[0023] In some embodiments of the present invention, the concentration of the soluble cerium salt solution is 8-20 mmol / L.

[0024] In some specific embodiments of the present invention, the concentration of the soluble cerium salt solution is 10-20 mmol / L.

[0025] In some examples of the present invention, the concentration of the soluble cerium salt solution is 10-12 mmol / L.

[0026] In some embodiments of the present invention, the volume of the soluble cerium salt solution is 10 to 30 mL.

[0027] In some embodiments of the present invention, the volume of the soluble cerium salt solution is 15-20 mL.

[0028] In some embodiments of the present invention, the copper sheet is immersed in the soluble cerium salt solution for 10 to 15 hours.

[0029] In some embodiments of the present invention, the copper sheet is immersed in the soluble cerium salt solution for 11 to 13 hours.

[0030] In some embodiments of the present invention, the immersion of the copper sheet in the soluble cerium salt solution is carried out under stirring conditions; the stirring speed is 200-400 r / min.

[0031] In some embodiments of the present invention, the rotation speed is 250-350 r / min.

[0032] In some embodiments of the present invention, the temperature of the heat treatment is 200-400°C.

[0033] In some embodiments of the present invention, the temperature of the heat treatment is 250-350°C.

[0034] In some embodiments of the present invention, the heat treatment time is 1 to 6 hours.

[0035] In some embodiments of the present invention, the heat treatment time is 2 to 6 hours.

[0036] In some specific embodiments of the present invention, the heat treatment time is 3 to 6 hours.

[0037] In some examples of the present invention, the heat treatment time is 3 to 4 hours.

[0038] In some embodiments of the present invention, the heat treatment is performed under aerobic conditions.

[0039] In some embodiments of the present invention, the heat treatment is performed in an air atmosphere.

[0040] In some embodiments of the present invention, the area of ​​the cathode and the anode immersed in the electrolyte is 3 to 7 cm 2 .

[0041] In some embodiments of the present invention, the area of ​​the cathode and the anode immersed in the electrolyte is 4 to 6 cm 2 .

[0042] In some specific embodiments of the present invention, the area of ​​the cathode and the anode immersed in the electrolyte is 4.5 to 6.5 cm 2 .

[0043] In some embodiments of the invention, the cathode comprises graphite.

[0044] In some embodiments of the present invention, the current density of the electrochemical oxidation is 2-6 mA / cm 2 .

[0045] In some embodiments of the present invention, the current density of the electrochemical oxidation is 3-5 mA / cm 2 .

[0046] In some embodiments of the present invention, the electrochemical oxidation time is 70 to 110 minutes.

[0047] In some embodiments of the present invention, the electrochemical oxidation time is 80 to 100 minutes.

[0048] In some specific embodiments of the present invention, the electrochemical oxidation time is 85 to 95 minutes.

[0049] In some embodiments of the present invention, the electrolyte includes at least one of a potassium bicarbonate solution and a sodium bicarbonate solution.

[0050] In some embodiments of the present invention, the concentration of the electrolyte is 0.05-0.5 mol / L.

[0051] In some specific embodiments of the present invention, the concentration of the electrolyte is 0.08-0.2 mol / L.

[0052] In some embodiments of the present invention, the soluble cerium salt includes cerium nitrate and / or cerium chloride.

[0053] In some embodiments of the present invention, the copper sheet is a pure copper sheet with a purity greater than 99.9%.

[0054] In some embodiments of the present invention, the copper sheet has a thickness of 0.1 to 0.2 mm.

[0055] In some embodiments of the present invention, the copper sheet is polished and washed.

[0056] In some embodiments of the present invention, the washing method is ultrasound.

[0057] In some specific embodiments of the present invention, the ultrasonic solution is a sodium hydroxide solution and / or a hydrochloric acid solution.

[0058] In some examples of the present invention, the ultrasonic step includes: ultrasonicating in a sodium hydroxide solution for 10 to 30 minutes, and then ultrasonicating in a hydrochloric acid solution for 10 to 30 minutes.

[0059] The third aspect of the present invention provides a use of the copper-based catalyst described in the first aspect of the present invention, or the copper-based catalyst obtained by the preparation method described in the second aspect of the present invention in catalytic reduction of carbon dioxide.

[0060] In some embodiments of the present invention, the copper-based catalyst is used to catalyze the reduction of carbon dioxide to produce ethylene.

[0061] The copper-based catalyst of the present invention has a wide range of raw materials, is low in price, and has a simple preparation method. The catalytic activity of the catalyst is improved by cerium doping, and its selectivity and stability are improved. The Faraday efficiency for preparing ethylene by electrochemical carbon dioxide reduction is relatively high.

[0062] In some embodiments of the present invention, the carbon dioxide reduction is electrochemical reduction.

[0063] In some embodiments of the present invention, the voltage of the electrochemical reduction is -0.6 to -1.5 V (vs. RHE).

[0064] In some specific embodiments of the present invention, the voltage of the electrochemical reduction is -0.9 to -1.1 V (vs. RHE).

[0065] In some embodiments of the present invention, when the copper-based catalyst is used to catalyze the reduction of carbon dioxide to produce ethylene, the copper-based catalyst is used as a working electrode; and a KHCO3 solution is used as an electrolyte.

[0066] In some specific embodiments of the present invention, the concentration of the KHCO3 solution is 0.4-0.6 mol / L.

[0067] Compared with the prior art, the present invention has the following beneficial effects:

[0068] (1) The present invention provides a copper-based catalyst, including copper, and copper oxide doped with cerium on the copper surface (CeCuOx, x is 0.5-1). The copper-based catalyst has the advantages of high specific surface area, rich reactive sites on the surface, excellent selectivity and catalytic activity, high stability, and doping with cerium can also improve the yield of the catalytic product. At the same time, the raw materials used are low in cost and widely available, and are suitable for large-scale production.

[0069] (2) The preparation method of the copper-based catalyst of the present invention is simple and convenient. It adopts a combination of electrochemical oxidation and immersion method. First, basic copper carbonate with a layered structure is formed on the copper surface, and then immersed in a soluble cerium salt solution. Electrostatic interaction is used to ensure uniform doping of cerium. After immersion, only further heat treatment is required to obtain a large-area catalyst, and no grinding, molding and other steps are required.

[0070] (3) The copper-based catalyst of the present invention has excellent catalytic activity, selectivity and stability, and is suitable for carbon dioxide reduction reaction, especially electrochemical reduction to produce ethylene. It has high Faraday efficiency and high ethylene yield, and is suitable for large-scale application of electrochemical carbon dioxide reduction to realize resource utilization of carbon dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1Schematic diagram of the preparation process of the copper-based catalyst of Example 1.

[0072] Figure 2 This is the XRD pattern of the copper-based catalyst of Example 1.

[0073] Figure 3 This is the element distribution diagram of the copper-based catalyst of Example 1.

[0074] Figure 4 This is a low-magnification SEM image of the copper-based catalyst of Example 1.

[0075] Figure 5 This is a high-magnification SEM image of the copper-based catalyst of Example 1.

[0076] Figure 6 This is the SEM image of cerium-doped copper oxide in the copper-based catalyst of Example 1.

[0077] Figure 7 The Faraday efficiency and ethylene yield of the copper-based catalyst of Example 1 for catalytic reduction of carbon dioxide to produce ethylene at different potentials.

[0078] Figure 8 The Faraday efficiency of the copper-based catalysts of Examples 1 to 4 for catalytic reduction of carbon dioxide to produce ethylene.

[0079] Fig. 9 The Faraday efficiency of the copper-based catalysts of Examples 1, 5 and 6 for catalytic reduction of carbon dioxide to produce ethylene.

[0080] Fig.10 The Faraday efficiency of the copper-based catalysts of Examples 1 and 7 for catalytic reduction of carbon dioxide to produce ethylene.

[0081] Fig.11 The Faraday efficiency and ethylene yield of ethylene produced by catalytic reduction of carbon dioxide by the catalyst of Comparative Example 1.

[0082] Fig.12 The Faraday efficiency and ethylene yield of the catalytic reduction of carbon dioxide to produce ethylene using pure copper sheets.

[0083] Fig.13 The yields of ethylene produced by the catalysts of Example 1 and Comparative Example 1 and pure copper sheets at different potentials.

[0084] Fig.14 This is a curve showing the change of current and Faraday efficiency over time in the accelerated decay life test of the copper-based catalyst of Example 1. DETAILED DESCRIPTION

[0085] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0086] Example 1

[0087] This embodiment provides a copper-based catalyst, including a copper substrate and cerium-doped copper oxide on the surface of the copper substrate; the mass content of cerium in the cerium-doped copper oxide is 3.6%.

[0088] like Figure 1 As shown in the preparation process diagram, the preparation method of the copper-based catalyst of this embodiment includes the following steps:

[0089] S1. Pure copper sheet (Cu, Cu>99.9%, thickness 0.1mm) was cut into 2×3cm size, polished with sandpaper, ultrasonicated in 1mol / L NaOH for 15min, ultrasonicated in 1mol / L HCl for 15min, and then washed with deionized water;

[0090] S2. Use potassium bicarbonate solution with a concentration of 0.1 mol / L as the electrolyte, pure copper sheet as the anode, and graphite sheet as the cathode; the pure copper sheet is used as the anode, and the area of ​​the electrode immersed in the electrolyte is 5 cm 2 ; Electrochemical oxidation reaction was carried out under stirring conditions with a current density of 4 mA / cm 2 , time is 90min; then use deionized water to wash away the residual solute on the surface, and use filter paper to absorb the excess water on the surface;

[0091] S3. The concentration of the cerium nitrate solution was 10 mmol / L and the volume was 15 mL. The electrochemically oxidized copper sheet obtained in step S3 was suspended in the cerium nitrate solution and stirred at a rate of 300 r / min for 12 h. The excess water on the surface was removed with filter paper;

[0092] S4. The catalyst precursor obtained in step S3 is placed in a muffle furnace and heat treated in an air atmosphere at 300° C. for 3 hours to obtain a copper-based catalyst, namely CeCuOx, where x is 0.5 to 1.

[0093] Example 2

[0094] This embodiment provides a copper-based catalyst, which is different from Embodiment 1 in that the mass content of cerium in the cerium-doped copper oxide is 1.23%.

[0095] The preparation method of the copper-based catalyst of this embodiment is different from the preparation method of Example 1 in that the concentration of the cerium nitrate solution is 2 mmol / L.

[0096] Example 3

[0097] This embodiment provides a copper-based catalyst, which is different from Embodiment 1 in that the mass content of cerium in the cerium-doped copper oxide is 2.28%.

[0098] The preparation method of the copper-based catalyst of this embodiment is different from the preparation method of Example 1 in that the concentration of the cerium nitrate solution is 5 mmol / L.

[0099] Example 4

[0100] This embodiment provides a copper-based catalyst, which is different from Embodiment 1 in that the mass content of cerium in the cerium-doped copper oxide is 5.26%.

[0101] The preparation method of the copper-based catalyst of this embodiment is different from the preparation method of Example 1 in that the concentration of the cerium nitrate solution is 20 mmol / L.

[0102] Example 5

[0103] This embodiment provides a copper-based catalyst, which is different from Embodiment 1 in that the mass content of cerium in the cerium-doped copper oxide is 4.51%.

[0104] The preparation method of the copper-based catalyst of this embodiment is different from the preparation method of Example 1 in that the heat treatment time is 1 hour.

[0105] Example 6

[0106] This embodiment provides a copper-based catalyst, which is different from Embodiment 1 in that the mass content of cerium in the cerium-doped copper oxide is 3.44%.

[0107] The preparation method of the copper-based catalyst of this embodiment is different from the preparation method of Example 1 in that the heat treatment time is 6 hours.

[0108] Example 7

[0109] This embodiment provides a copper-based catalyst, which is different from Embodiment 1 in that the mass content of cerium in the cerium-doped copper oxide is 4.25%.

[0110] The method for preparing the copper-based catalyst of this embodiment is different from the method for preparing the copper-based catalyst of Embodiment 1 in that the cerium nitrate solution is replaced by a cerium chloride solution.

[0111] Comparative Example 1

[0112] This comparative example provides a method for preparing a catalyst, which is different from the preparation method of Example 1 in that the copper sheet after ultrasound is directly subjected to electrochemical oxidation and heat treatment without being immersed in a cerium nitrate solution. The obtained catalyst is recorded as CuOx, where x is 0.5-1.

[0113] Performance Testing

[0114] The catalysts obtained in the above embodiments and comparative examples and the pure copper sheet with a purity of >99.9% and a thickness of 0.1 mm were subjected to electrochemical catalytic performance tests. The electrochemical tests were conducted at 25°C and 100 kPa pressure in a 0.5 M KHCO3 solution saturated with carbon dioxide. Carbon dioxide was continuously introduced during the test to achieve saturation. The test used a three-electrode system, with a Ti mesh coated with Ru-Ir oxide as the anode, a saturated calomel electrode as the reference electrode, and the catalyst or copper sheet of the embodiments and comparative examples as the working electrode. During the reaction, the solution was extracted every 13 minutes to characterize the gas phase product by gas chromatography.

[0115] Combine the following Figures 2 to 12 The performance test results of the present invention are described in detail:

[0116] Figure 2 is the XRD pattern of the copper-based catalyst of Example 1, Figure 3 is the element distribution diagram of the copper-based catalyst of Example 1, Figure 4 This is a low-power SEM image of the copper-based catalyst of Example 1. Figure 5 This is a high-magnification SEM image of the copper-based catalyst of Example 1. Figure 6 is a SEM image of cerium-doped copper oxide in the copper-based catalyst of Example 1. Figure 2 From the XRD pattern, it can be seen that CeCuOx is composed of Cu and CuO phases, and no Ce compound phase is observed. Figure 3 The element distribution shows that Cu and Ce are distributed in two different regions, proving that the cerium-doped copper oxide on the surface is divided into Ce-poor and Ce-rich phases. The surface structure of the copper-based catalyst is shown in Figure 2. Figure 4 and 5 As shown, it can be seen that the surface of CeCuOx is composed of agglomerated nano-morphology, with a cerium content of 3.6% and a thickness of 2 μm ( Figure 6 ). Under a high-power electron microscope ( Figure 5 ) shows that each agglomerate of the copper-based catalyst has a fine morphology of graded nanoparticles, indicating that the catalyst has a large specific surface area, which is beneficial to the improvement of catalytic performance.

[0117] Figure 7 The Faraday efficiency and ethylene yield of the copper-based catalyst in Example 1 for catalytic reduction of carbon dioxide to produce ethylene at different potentials. Figure 7 It can be seen that CeCuOx produces ethylene, a small amount of carbon monoxide and hydrogen in the reduction of carbon dioxide. At a voltage of -0.93V vs. RHE, the copper-based catalyst CeCuOx achieves the best Faraday efficiency for the reduction of carbon dioxide to ethylene, and the best yield of carbon dioxide reduction to ethylene is achieved at -1.03V.

[0118] Figure 8 The Faraday efficiency of the copper-based catalysts in Examples 1 to 4 for catalytic reduction of carbon dioxide to produce ethylene. Different concentrations of cerium nitrate solutions were used as the cerium-doped medium. Figure 8 The results show that when the concentration of cerium nitrate solution is controlled to 10 mmol / L, the copper-based catalyst CeCuOx obtained has a higher Faraday efficiency for the reduction of ethylene by carbon dioxide than samples with other concentrations.

[0119] Fig. 9 The Faraday efficiency of the copper-based catalysts in Examples 1, 5, and 6 for catalytic reduction of carbon dioxide to produce ethylene. The performance of the catalysts obtained by different heat treatment times was tested. Fig. 9 The results show that when the heat treatment time is controlled to 3h, the obtained CeCuOx has a higher Faraday efficiency for the reduction of ethylene by carbon dioxide than the samples with other heat treatment times.

[0120] Fig.10 The Faraday efficiency of the copper-based catalysts in Examples 1 and 7 for catalytic reduction of carbon dioxide to produce ethylene. Using cerium chloride as a cerium source, the obtained copper-based catalysts were tested for performance. Fig.10 It can be seen from the test results that CeCuOx obtained by soaking in cerium nitrate solution has a higher Faraday efficiency for the reduction of ethylene by carbon dioxide than CeCuOx obtained by soaking in cerium chloride.

[0121] Fig.11 The Faraday efficiency and yield of ethylene produced by catalytic reduction of carbon dioxide by the catalyst of Comparative Example 1 are: Fig.12 The Faraday efficiency and yield of ethylene produced by catalytic reduction of carbon dioxide by pure copper sheet. Fig.11 and Fig.12 It can be seen that the Faraday efficiency and yield of ethylene of the copper-based catalyst at different potentials are higher than those of CuOx and copper sheets without cerium doping, which proves that the cerium doping of the present invention has an improving effect on the selectivity of ethylene.

[0122] Fig.13 The yields of ethylene produced by the catalysts of Example 1 and Comparative Example 1 and the pure copper sheet at different potentials. Fig.13 It can be seen that at all potentials, the copper-based catalyst of Example 1 has a higher ethylene yield than the copper sheet and the CuOx of Comparative Example 1, which proves that the incorporation of cerium is beneficial to the process of catalyzing the reduction of carbon dioxide to produce ethylene.

[0123] Fig.14 The curve of the current and the Faraday efficiency of the copper-based catalyst of Example 1 in the accelerated decay life test over time. Fig.14As can be seen from the figure, the CeCuOx catalyst has a current density of 100 mA cm-1 at a potential of -0.93 V vs RHE and undergoes 8 cycles of about 220 hours of accelerated decay life test of on-off circuit. -2 At the same time, the Faraday efficiency of generating ethylene is stable at around 55%, which proves that the copper-based catalyst of the present invention has high stability and is stable in generating ethylene.

[0124] In summary, the present invention uses copper sheet as a substrate and adopts a simple electrochemical oxidation-immersion-heat treatment composite method to prepare a copper-based catalyst with high carbon dioxide reduction Faraday efficiency for preparing ethylene, high ethylene yield, and high selectivity and stability. Combined with the above performance test analysis, it can be seen that when the concentration of cerium nitrate is 10mmol / L, the copper-based catalyst of the present invention has good selectivity and catalytic activity for preparing ethylene by carbon dioxide reduction. In a 0.5M KHCO3 solution saturated with carbon dioxide, the potential of the copper-based catalyst with the highest Faraday efficiency for producing ethylene is -0.93V, corresponding to a Faraday efficiency of 55%, and the ethylene yield is 3.3mmol h -1 cm -2 At the same time, at a potential of -0.83 to -1.13 V, the maximum yield of ethylene was 3.7 mmol h -1 cm -2 (potential is -1.03V), the Faraday efficiency is stable at more than 50%, which is higher than the existing copper-based catalyst for reducing ethylene with carbon dioxide. It can be seen that the copper-based catalyst of the present invention has excellent catalytic activity, and has obvious advantages over the Faraday efficiency of less than 40% of the copper-based catalyst in the prior art, and is very suitable for large-scale applications of electrochemical carbon dioxide reduction.

[0125] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A copper-based catalyst, characterized in that A method for preparing a cerium-doped copper oxide substrate comprising a substrate and a cerium-doped copper oxide on a surface of the substrate; wherein the substrate comprises copper; The mass content of cerium in the cerium-doped copper oxide is 1-6%.

2. The copper-based catalyst according to claim 1, characterized in that The thickness of the cerium-doped copper oxide on the surface of the substrate is 1 to 3 μm.

3. A method for preparing the copper-based catalyst according to claim 1 or 2, characterized in that: The steps include: The copper sheet is used as the anode and immersed in the electrolyte together with the cathode for electrochemical oxidation; Soaking the electrochemically oxidized copper sheet in a soluble cerium salt solution to obtain a catalyst precursor; The catalyst precursor is heat-treated to obtain the copper-based catalyst.

4. The preparation method according to claim 3, characterized in that: The concentration of the soluble cerium salt solution is 8 to 20 mmol / L; And / or, the copper sheet is immersed in the soluble cerium salt solution for 10 to 15 hours.

5. The preparation method according to claim 3, characterized in that: The temperature of the heat treatment is 200-400°C; And / or, the heat treatment time is 2 to 6 hours; And / or, the heat treatment is performed under aerobic conditions.

6. The preparation method according to claim 3, characterized in that: The area of ​​the anode and the cathode immersed in the electrolyte is 3 to 7 cm 2 ; And / or, the cathode comprises graphite.

7. The preparation method according to claim 3 or 6, characterized in that: The current density of the electrochemical oxidation is 2-6 mA / cm 2 ; And / or, the electrochemical oxidation time is 70 to 110 minutes.

8. The preparation method according to claim 3, characterized in that: The electrolyte includes at least one of a potassium bicarbonate solution and a sodium bicarbonate solution; and / or the concentration of the electrolyte is 0.05 to 0.5 mol / L; And / or, the soluble cerium salt includes cerium nitrate and / or cerium chloride.

9. Use of the copper-based catalyst according to claim 1 or 2, or the copper-based catalyst obtained by the preparation method according to any one of claims 3 to 8 in catalytic reduction of carbon dioxide.

10. The use according to claim 9, characterized in that: The copper-based catalyst is used for catalyzing the reduction of carbon dioxide to produce ethylene.