Functional polyester, functional polyester fiber, preparation method and application
During the preparation of polyester fiber, the contact reaction and esterification reaction of aromatic dibasic acid and ethylene glycol and the use of antioxidants are solved, and the problem of poor dyeing performance of polyester fibers is achieved. Functional polyester fiber with dyeing rate and hydrophilic properties, suitable for industrial production.
Patent Information
- Application Number
- CN202310490549.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-05
AI Technical Summary
The dyeing performance of existing polyester fibers is poor, resulting in fewer high-value-added products in industrial production, and dye-modified polyesters have complex reactions due to the introduction of monomers, which affects the structure and performance of copolyesters.
By mixing aromatic dibasic acid, ethylene glycol and catalyst for contact reaction, polyethylene glycol-ethylene glycol solution is added for esterification and polycondensation reaction, the reaction conditions are controlled to improve the dyeing and hydrophilic properties, and at the contact Antioxidants are added to the reaction to stabilize the product.
It has achieved high dyeing rate and good hydrophilic properties of functional polyester fibers, can resist lint and pilling, and has good processing performance, which significantly improves dyeing performance and market prospects.
Smart Images

Figure BDA0004210212630000181
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer chemical industry, and in particular to a functional polyester, a functional polyester fiber, and a preparation method and application thereof. Background Art
[0002] Faced with increasingly severe market conditions, research on polyester modification has been carried out for many years to expand polyester applications and cope with industry competition. Although industrial modified products and output have increased in recent years, there has been no breakthrough progress. The development of modified polyester products requires making up for performance shortcomings while avoiding the decline of other properties. Therefore, ensuring production operation rate or maintaining processing performance has become a topic of continuous in-depth research.
[0003] Polyethylene glycol terephthalate (PET) fiber has the characteristics of high strength, good dimensional stability, and crispness without wrinkles. It has always been the main raw material for clothing products. However, since PET can only use disperse dyes and requires high temperature and high pressure dyeing conditions to improve the dyeing rate, improving the dyeability of PET has always been a hot topic of continuous concern. Dyeing-modified PET products can often improve the fiber's hygroscopicity and anti-pilling performance, which is one of the important directions for the current industrial structure adjustment of polyester manufacturers. Improving dyeability has always been the main research direction of polyester modification. At present, a lot of work has been carried out in the field of disperse dyes at normal pressure and cationic dyeability. The method adopted is to introduce groups that can bind to dye molecules on the PET molecular chain, or introduce monomers that slow down polyester crystallization and facilitate the entry of dyes into the amorphous region.
[0004] Chinese Patent 201310420953.9 synthesizes a copolyether ester (COPEET) composed of polyethylene terephthalate, polyethylene isophthalate and aliphatic polyether flexible chain segments, using it as the island component. The ultrafine fibers made by the sea-island yarn method can achieve normal pressure deep dyeing with disperse dyes. The invention does not conduct in-depth research on the process of copolyether ester, and the glass transition temperature below 65°C may cause the problem of drawing and sticking in the pre-spinning process.
[0005] Chinese patent application 202111041468.1 discloses a method for preparing a copolyester dyeable at normal pressure with medium-high viscosity disperse dyes, in which polycaprolactone diol is used to replace or partially replace polyethylene glycol. Polycaprolactone diol has high thermal stability, but the condensation reaction temperature of the copolyester is as high as 292°C, which can easily lead to an increase in polyester side reactions, which is not conducive to subsequent spinning operations.
[0006] Chinese Patent No. 201611160113.3 discloses an aromatic polyester-aliphatic polyester block copolyester fiber, which is formed by condensation polymerization of ethylene terephthalate oligomers and aliphatic polydiacid diol ester polyols. In the actual polymerization process, the dibasic acid in the aliphatic polydiacid diol ester polyol in the invention is a straight-chain aliphatic dibasic acid, which is succinic acid, adipic acid or sebacic acid. The aliphatic dibasic acid has a short molecular chain, so under the condition of high content and the absence of antioxidants and stabilizers, there will be an increase in small molecules caused by thermal oxidation degradation, resulting in defects in the spinning process.
[0007] Chinese patent 200910048274.7 discloses a method for preparing polyester pearl fibers dyeable at room temperature and pressure, wherein the pearls are sheared and ground to obtain coarse pearl powder, and then the coarse pearl powder, a heat stabilizer, an antioxidant and an emulsifier are mixed and added to polyester chips dyeable at room temperature and pressure, and then melt-extruded to obtain nano-pearl polyester chips. The blending method used in the invention is difficult to ensure uniformity, which affects its subsequent use.
[0008] There are many studies on the modification of the dyeing properties of polyester fiber products, but there are few high-value-added products that are truly used in industrial production. The reason is that the reaction of dyed modified polyester is more complicated due to the introduction of monomers. The monomer addition process, esterification process, and polycondensation process will affect the structure and properties of copolyester. Therefore, while ensuring the conventional excellent performance of polyester, developing functional polyester products that are easy to dye and hydrophilic has significant market prospects and environmental benefits. Summary of the invention
[0009] The purpose of the present invention is to overcome the problem of poor dyeing performance of polyester fibers and subsequent products in the prior art, and to provide a functional polyester, a functional polyester fiber and a preparation method and application thereof. The functional polyester fiber has good dyeing performance and hydrophilicity, and can resist pilling and fuzzing.
[0010] In order to achieve the above object, the first aspect of the present invention provides a functional polyester fiber, wherein the dye uptake rate of the functional polyester fiber is greater than 94% and the K / S value is greater than 26.
[0011] Preferably, the moisture regain of the functional polyester fiber is 0.49-0.56%.
[0012] The second aspect of the present invention provides a method for preparing a functional polyester, comprising the following steps:
[0013] (1) mixing an aromatic dibasic acid, ethylene glycol and a catalyst to carry out a contact reaction I;
[0014] (2) subjecting the product obtained from the contact reaction I to a contact reaction II with a polyethylene glycol-ethylene glycol solution.
[0015] Preferably, the aromatic dibasic acid includes a first aromatic dibasic acid and a second aromatic dibasic acid, and the catalyst is an antimony catalyst.
[0016] Preferably, the first aromatic dibasic acid is terephthalic acid; the second aromatic dibasic acid is selected from at least one of isophthalic acid, 2,6-naphthalene dicarboxylic acid and 4,4'-biphenyl dicarboxylic acid, more preferably isophthalic acid; the antimony catalyst is selected from at least one of ethylene glycol antimony, antimony trioxide and antimony acetate.
[0017] Preferably, the weight ratio of the first aromatic dibasic acid, the second aromatic dibasic acid, the ethylene glycol and the polyethylene glycol-ethylene glycol solution is 1:0.05-0.10:0.59-0.65:0.06-0.13.
[0018] Preferably, the concentration of polyethylene glycol in the polyethylene glycol-ethylene glycol solution is 30-50% by weight.
[0019] Preferably, the number average molecular weight of the polyethylene glycol is 1000-5000, more preferably 2000.
[0020] Preferably, in step (1), the conditions of the contact reaction I include at least: a temperature of 245-265° C. and a relative pressure of 0.24-0.26 MPa; and the conditions for the termination of the contact reaction I include at least: an acid value of the product of the contact reaction I of 20-60 mg KOH / g.
[0021] Preferably, in step (2), the process of the contact reaction II comprises: subjecting the product obtained from the contact reaction I to an esterification reaction and a polycondensation reaction with a polyethylene glycol-ethylene glycol solution.
[0022] Preferably, the conditions of the esterification reaction include at least: a temperature of 225-240° C., a relative pressure of 0.24-0.26 MPa, and a time of 20-60 min.
[0023] Preferably, the polycondensation reaction process comprises: subjecting the product of the esterification reaction to a preliminary polycondensation reaction to obtain a prepolymerization product, and subjecting the prepolymerization product to a final polycondensation reaction.
[0024] Preferably, the conditions of the pre-polycondensation reaction at least include: an absolute pressure of 0.1-100 kPa.
[0025] Preferably, the conditions for the final polycondensation reaction include at least: a temperature of 282-286° C. and an absolute pressure of 0.01-0.5 kPa; and the conditions for the end of the final polycondensation reaction process include at least: a stirring current reaches a preset value.
[0026] Preferably, the method further comprises: adding an auxiliary agent during the contact reaction I.
[0027] Preferably, the auxiliary agent is an antioxidant, more preferably a phenolic antioxidant.
[0028] Preferably, the weight ratio of the auxiliary agent to the aromatic dibasic acid is 1:1650-1700.
[0029] The third aspect of the present invention provides a functional polyester obtained by the preparation method described in the second aspect.
[0030] Preferably, the functional polyester has an intrinsic viscosity of 0.50-0.69 dL / g and a glass transition temperature of 60°C-73°C.
[0031] The fourth aspect of the present invention provides a functional polyester fiber obtained by spinning the functional polyester described in the third aspect.
[0032] The fifth aspect of the present invention provides use of the functional polyester fiber described in the first aspect, the functional polyester fiber provided in the fourth aspect and / or the functional polyester described in the third aspect in the preparation of clothing products.
[0033] Through the above technical solution, the beneficial effects of the present invention are:
[0034] The functional polyester fiber provided by the present invention has a high dye uptake rate, is easy to dye, and has significant market prospects and environmental benefits. The preparation method of the functional polyester provided by the present invention comprises the following steps: firstly, an aromatic dibasic acid, ethylene glycol and a catalyst are mixed to carry out a contact reaction I, and a polyethylene glycol-ethylene glycol solution is added to the product obtained by the contact reaction I, so that the product obtained by the contact reaction I can be cooled down to prevent the polyethylene glycol monomer from entering the reaction system and undergoing a degradation reaction due to excessive temperature, and the product obtained by the contact reaction I can be diluted to avoid the reaction unevenness caused by excessive product viscosity, so that the contact reaction II can be carried out more smoothly, thereby improving the dyeing performance and hydrophilicity of the functional polyester, and having the effects of anti-pilling and anti-pilling, and having good processing performance.
[0035] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0036] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0037] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0038] A first aspect of the present invention provides a functional polyester fiber, wherein the dye uptake rate of the functional polyester fiber is greater than 94% and the K / S value is greater than 26.
[0039] In the present invention, the functional polyester fiber has excellent dyeing performance. The specific testing method is: the functional polyester fiber fabric is dyed with 3 wt% disperse blue dye at a bath ratio of 1:30 and a temperature of 100° C. for 60 minutes, and the dyeing rate and K / S value of the fabric after dyeing are tested.
[0040] In the present invention, dye uptake and K / S value are important indicators for evaluating fabric dyeing performance and are used to characterize dyeing depth. Dye uptake refers to the ratio of the amount of dye dyed onto the fiber to the total amount of dye put into the dye bath during the dyeing process, which is often expressed as a percentage and is also called dye uptake percentage. Dye uptake is obtained by measuring the dye concentration in the original dye solution and the dye concentration in the dye bath after a specific dyeing time, and then calculating the difference between the two. The Kubelka-Munk dyeing depth equation establishes a certain functional relationship between the absorption coefficient K and the scattering coefficient S of the measured object and the concentration C of the colored substance in the solid sample. The larger the K / S value obtained by calculation, the darker the surface color of the solid sample, that is, the higher the concentration of the colored substance, the better the dyeing performance of the dye.
[0041] According to the present invention, preferably, the moisture regain of the functional polyester fiber is 0.49-0.56%.
[0042] The second aspect of the present invention provides a method for preparing a functional polyester, comprising the following steps:
[0043] (1) mixing an aromatic dibasic acid, ethylene glycol and a catalyst to carry out a contact reaction I;
[0044] (2) subjecting the product obtained from the contact reaction I to a contact reaction II with a polyethylene glycol-ethylene glycol solution.
[0045] The inventors of the present invention found in the process of research that since polyethylene glycol is composed of polyether segments and has poor thermal stability, the product obtained by contact reaction I can be cooled by adding polyethylene glycol and ethylene glycol into a mixed solution to the product obtained by contact reaction I for contact reaction II, thereby preventing the polyethylene glycol monomer from entering the reaction system and undergoing degradation reaction due to excessive temperature; polyethylene glycol is solid, and heating it and dissolving it in ethylene glycol to prepare a mixed solution can enter the reaction system more uniformly and stably, thereby ensuring the stability of the monomer content in the product, and a certain amount of ethylene glycol added to contact reaction II can dilute the product of contact reaction I and prevent the reaction from being unevenly caused by excessive viscosity. Moreover, the functional polyester prepared by the above method has excellent dyeing performance and hydrophilicity, strong spinnability, and can give the functional polyester fiber obtained by spinning it anti-pilling and anti-pilling effects.
[0046] According to the present invention, preferably, the aromatic dibasic acid includes a first aromatic dibasic acid and a second aromatic dibasic acid, and the catalyst is an antimony catalyst.
[0047] According to the present invention, preferably, the first aromatic dibasic acid is terephthalic acid; the second aromatic dibasic acid is selected from at least one of isophthalic acid, 2,6-naphthalene dicarboxylic acid and 4,4'-biphenyl dicarboxylic acid, more preferably isophthalic acid; the antimony catalyst is selected from at least one of ethylene glycol antimony, antimony trioxide and antimony acetate.
[0048] In the present invention, the amount of the catalyst can be selected according to the performance requirements of the functional polyester. Specifically, the amount of the catalyst is 0.037-0.042 wt % relative to the weight of the aromatic dibasic acid.
[0049] According to the present invention, preferably, the weight ratio of the first aromatic dibasic acid, the second aromatic dibasic acid, the ethylene glycol and the polyethylene glycol-ethylene glycol solution is 1:0.05-0.10:0.59-0.65:0.06-0.13.
[0050] According to the present invention, preferably, the concentration of polyethylene glycol in the polyethylene glycol-ethylene glycol solution is 30-50% by weight.
[0051] According to the present invention, preferably, the number average molecular weight of the polyethylene glycol is 1000-5000, more preferably 2000.
[0052] In the present invention, the first aromatic dibasic acid, the second aromatic dibasic acid, ethylene glycol, polyethylene glycol and the catalyst can be purchased commercially or prepared by the preparation method disclosed in the prior art.
[0053] According to the present invention, in order to further improve the reaction rate of contact reaction I and the yield of the product, preferably, the conditions of the contact reaction I at least include: a temperature of 245-265°C and a relative pressure of 0.24-0.26MPa; the conditions for the termination of the contact reaction I process at least include: the acid value of the product of the contact reaction I is 20-60mg KOH / g.
[0054] According to the present invention, in order to further improve the reaction rate of contact reaction II and the yield of the product, preferably, in step (2), the process of contact reaction II includes: subjecting the product obtained from contact reaction I to esterification reaction and polycondensation reaction with polyethylene glycol-ethylene glycol solution.
[0055] According to the present invention, in order to further improve the reaction rate and product yield of the esterification reaction, preferably, the conditions of the esterification reaction include at least: temperature of 225-240° C., relative pressure of 0.24-0.26 MPa, and time of 20-60 min.
[0056] According to the present invention, preferably, the polycondensation reaction process comprises: subjecting the product of the esterification reaction to a preliminary polycondensation reaction to obtain a prepolymer product, and subjecting the prepolymer product to a final polycondensation reaction. The inventors have found that under this preferred embodiment, it is beneficial to shorten the polycondensation reaction time, reduce the residence time of polyethylene glycol in the reaction system, and thus improve the stability of the structure and performance of the functional polyester.
[0057] In the present invention, the pre-polycondensation reaction is a gradually increasing temperature stage, which gradually increases from the temperature at the end of the esterification reaction to the final polycondensation reaction temperature. According to the present invention, in order to further improve the stability of the structure and performance of the functional polyester, preferably, the conditions of the pre-polycondensation reaction include at least: an absolute pressure of 0.1-100 kPa.
[0058] According to the present invention, in order to further improve the stability of the structure and performance of the functional polyester, preferably, the conditions for the final polycondensation reaction include at least: a temperature of 282-286°C and an absolute pressure of 0.01-0.5 kPa; the conditions for the end of the final polycondensation reaction process include at least: the stirring current reaches a preset value.
[0059] In the present invention, the preset value of the stirring current is the rated current value of the reactor used. Different reactors have different rated current values.
[0060] According to the present invention, preferably, the method further comprises: adding an auxiliary agent during the contact reaction I.
[0061] According to the present invention, preferably, the auxiliary agent is an antioxidant, more preferably a phenolic antioxidant. The inventors have found that under this preferred embodiment, the phenolic antioxidant can prevent or inhibit the chain initiation reaction and the chain growth reaction by capturing peroxyl radicals, thereby preventing the free radical chain reaction and achieving the purpose of preventing oxidation.
[0062] In the present invention, there is no particular limitation on the type of the phenolic antioxidant, and the phenolic antioxidant may be any conventional phenolic antioxidant in the art, for example, Antioxidant 1010.
[0063] According to the present invention, preferably, the weight ratio of the auxiliary agent to the aromatic dibasic acid is 1:1650-1700.
[0064] In the present invention, the method for preparing the functional polyester further comprises: extruding, pelletizing and drying the product of the final polycondensation reaction, wherein the extrusion, pelletizing and drying methods can be conventionally used in conventional manners and equipment.
[0065] The third aspect of the present invention provides a functional polyester obtained by the preparation method described in the second aspect.
[0066] According to the present invention, preferably, the functional polyester has an intrinsic viscosity of 0.50-0.69 dL / g and a glass transition temperature of 60°C-73°C.
[0067] The fourth aspect of the present invention provides a functional polyester fiber obtained by spinning the functional polyester described in the third aspect.
[0068] In the present invention, there is no particular limitation on the spinning conditions. Preferably, the spinning temperature is 286-290° C. and the spinning speed is 2800-3200 m / min. The inventors have found that under this preferred embodiment, the functional polyester melt has good spinning performance.
[0069] The fifth aspect of the present invention provides use of the functional polyester fiber described in the first aspect, the functional polyester fiber described in the fourth aspect and / or the functional polyester described in the third aspect in the preparation of clothing products.
[0070] According to a particularly preferred embodiment of the present invention, there is provided a method for preparing a functional polyester fiber, comprising the following steps:
[0071] (1) mixing a first aromatic dibasic acid, a second aromatic dibasic acid, ethylene glycol, a catalyst and an auxiliary agent, and performing a contact reaction I at a temperature of 245-265° C. and a relative pressure of 0.24-0.26 MPa, until the acid value of the product of the contact reaction I is 20-60 mg KOH / g;
[0072] (2) subjecting the product obtained from the contact reaction I in step (1) and a polyethylene glycol-ethylene glycol solution having a polyethylene glycol concentration of 30-50 wt % to an esterification reaction at a temperature of 225-240° C. and a relative pressure of 0.24-0.26 MPa for 20-60 min;
[0073] (3) subjecting the product of the esterification reaction in step (2) to a pre-polycondensation reaction at a heating rate of 100 kPa and an absolute pressure of 0.1-100 kPa to obtain a pre-polycondensation product, and subjecting the pre-polycondensation product to a final polycondensation reaction at a temperature of 282-286° C. and an absolute pressure of 0.01-0.5 kPa until the stirring current reaches a preset value, thereby obtaining a functional polyester;
[0074] (4) spinning the functional polyester obtained in step (3) at a spinning temperature of 286-290° C. and a spinning speed of 2800-3200 m / min to obtain functional polyester fibers;
[0075] The first aromatic dibasic acid is terephthalic acid, the second aromatic dibasic acid is isophthalic acid, the catalyst is ethylene glycol antimony, the auxiliary agent is antioxidant 1010, and the number average molecular weight of polyethylene glycol is 2000; the weight ratio of the first aromatic dibasic acid, the second aromatic dibasic acid, ethylene glycol and polyethylene glycol-ethylene glycol solution is 1:0.05-0.10:0.59-0.65:0.06-0.13, and the weight ratio of the auxiliary agent to the total weight of the first aromatic dibasic acid and the second aromatic dibasic acid is 1:1650-1700; relative to the total weight of the first aromatic dibasic acid and the second aromatic dibasic acid, the amount of ethylene glycol antimony is 0.037-0.042 weight%.
[0076] In the above preferred embodiment, the prepared functional polyester has excellent dyeing property, hydrophilic property and spinning property.
[0077] In the present invention, the conventional polyester can be a commercially available common polyester, or a polyester prepared by a conventional method in the art. Exemplarily, the preparation method of the conventional fiber comprises the following steps: ethylene glycol antimony catalyst, terephthalic acid (PTA) and ethylene glycol (EG) are mixed in a weight ratio of 1:2800-3200:1600-2000, and a conventional esterification reaction is carried out under the conditions of a gauge pressure of 0.2-0.3MPa and a temperature of 200-300°C; after the esterification reaction is completed, a pre-polycondensation reaction is carried out at 260-275°C for 40-50min, and finally the polycondensation reaction temperature is controlled to be 270-285°C for a final polycondensation reaction, the absolute pressure is 0.01-0.5kPa, and the cumulative polycondensation time is 100-120min after the stirring current of the reactor reaches the set value, and the melt is extruded by a melt pump, pelletized, and dried to obtain a conventional polyester.
[0078] The present invention is described in detail below with reference to the embodiments, but the scope of the present invention is not limited thereby.
[0079] In the following examples and comparative examples, the raw materials are all commercially available.
[0080] The intrinsic viscosity, diethylene glycol content and b value are tested according to 5.1 of GB / T14190-2017 Test Method for Fiber-Grade Polyester Chips.
[0081] The glass transition temperature (Tg) is calculated by differential scanning calorimetry (DSC) test, and the specific process is: under nitrogen protection, DSC thermal analysis is used to increase the temperature from 25°C to 290°C at a heating rate of 20°C / min, maintain for 5 minutes, then cool to 25°C at a rate of 400°C / min, then increase the temperature from 25°C to 290°C at a heating rate of 20°C / min, maintain for 5 minutes, and finally cool to 100°C at a rate of 20°C / min, and calculate the glass transition temperature Tg according to the second heating curve.
[0082] The fiber moisture regain test is carried out in accordance with GB / T 6503-2008 "Test method for moisture regain of chemical fibers".
[0083] The specific process of the test method for the dyeing performance of the garters is: using 3 wt % disperse blue dye at a bath ratio of 1:30 and a temperature of 100° C. for a holding time of 60 minutes, and testing the dyeing rate and K / S value of the garters after dyeing.
[0084] Example 1
[0085] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 241g of isophthalic acid (IPA), 3000g of ethylene glycol (EG), 1.99g of ethylene glycol antimony catalyst and 3.01g of antioxidant 1010 were added, and the first stage esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the first stage esterification reaction, the acid value of the esterified product was tested to be 38mg. The reaction kettle was cooled, and 361 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was added, and the second esterification reaction was continued at a temperature of 230°C for 40 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 284°C and an absolute pressure of 0.01-0.5 kPa. The final polycondensation reaction was carried out until the stirring current of the reaction kettle reached the set value and the final polycondensation time was 102 min to obtain a melt; the melt was extruded through a melt pump, pelletized, and dried to obtain 6011.1 g of functional polyester.
[0086] Example 2
[0087] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 372g of isophthalic acid (IPA), 3000g of ethylene glycol (EG), 2.05g of ethylene glycol antimony catalyst and 3.10g of antioxidant 1010 were added, and the first stage esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the first stage esterification reaction, the acid value of the esterified product was tested to be 41mg. The reaction kettle was cooled, and 434 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was added, and the second esterification reaction was continued at a temperature of 225°C for 60 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 284°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the final polycondensation time was 75 min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 6199.1 g of functional polyester.
[0088] Example 3
[0089] In a 20L general polymerization reactor, 5350g of terephthalic acid (PTA), 408g of isophthalic acid (IPA), 3200g of ethylene glycol (EG), 2.15g of ethylene glycol antimony catalyst and 3.40g of antioxidant 1010 were added, and the first stage esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 245°C. At the end of the first stage esterification reaction, the acid value of the esterified product was tested to be 59mg. The reaction kettle was cooled, and 454 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 30 wt% was added, and the second esterification reaction was continued at a reaction temperature of 235°C for 40 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 282°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the final polycondensation time was 61 min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 6796.1 g of functional polyester.
[0090] Example 4
[0091] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 244g of isophthalic acid (IPA), 3100g of ethylene glycol (EG), 2.09g of ethylene glycol antimony catalyst and 3.04g of antioxidant 1010 were added, and the first stage esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the first stage esterification reaction, the acid value of the esterified product was tested to be 40mg. The reaction kettle was cooled, and 608 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 40 wt% was added, and the second esterification reaction was continued at a temperature of 240°C for 35 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 286°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the final polycondensation time was 78 min to obtain a melt, and the melt was extruded, pelletized and dried by a melt pump to obtain 6077.21 g of functional polyester.
[0092] Example 5
[0093] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 242g of isophthalic acid (IPA), 3100g of ethylene glycol (EG), 2.00g of ethylene glycol antimony catalyst and 3.02g of antioxidant 1010 were added, and the first stage esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 265°C. At the end of the first stage esterification reaction, the acid value of the esterified product was tested to be 22mg. The reaction kettle was cooled, and 423 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was added, and the second esterification reaction was continued at a temperature of 230°C for 40 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 284°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the final polycondensation time was 81 min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 6043.2 g of functional polyester.
[0094] Example 6
[0095] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 435g of isophthalic acid (IPA), 3100g of ethylene glycol (EG), 2.13g of ethylene glycol antimony catalyst and 3.10g of antioxidant 1010 were added, and the first stage esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the first stage esterification reaction, the acid value of the esterified product was tested to be 43mg. The reaction kettle was cooled, and 310 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was added, and the second esterification reaction was continued at a temperature of 230°C for 40 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 284°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the final polycondensation time was 117 min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 6209.9 g of functional polyester.
[0096] Example 7
[0097] The functional polyester was prepared according to the method of Example 1, except that 361 g of the polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was replaced by 902 g of the polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 20 wt%, and the final polycondensation time was 97 min.
[0098] Example 8
[0099] The functional polyester was prepared according to the method of Example 1, except that the time of the second esterification reaction was replaced with 90 min and the final polycondensation time was 109 min.
[0100] Example 9
[0101] The functional polyester was prepared according to the method of Example 1, except that the temperature of the final polycondensation reaction was replaced with 279° C. and the final polycondensation time was 140 min.
[0102] Example 10
[0103] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 598g of isophthalic acid (IPA), 3100g of ethylene glycol (EG), 2.20g of ethylene glycol antimony catalyst, and 3.32g of antioxidant 1010 were added. The first stage of esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the first stage of esterification reaction, the acid value of the esterified product was tested to be 41mg. The reaction kettle was cooled, and 797 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was added, and the second esterification reaction was continued at a temperature of 230°C for 40 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 284°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the cumulative polycondensation time was 115 min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 6642.0 g of functional polyester.
[0104] Comparative Example 1
[0105] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG) and 1.66g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, the acid value of the esterified product was tested to be 38mg KOH / g. The temperature was gradually increased, and a pre-polycondensation reaction was carried out for 45min under the condition of an absolute pressure of 0.1-100kPa, and a final polycondensation reaction was carried out under the conditions of a temperature of 279°C and an absolute pressure of 0.01-0.5kPa. After the stirring current of the reactor reached the set value, the final polycondensation time was 112min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 5783.1g of polyester (hereinafter referred to as conventional polyester).
[0106] Comparative Example 2
[0107] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 241g of isophthalic acid (IPA), 3000g of ethylene glycol (EG), 361g of a 50% polyethylene glycol (PEG2000) / ethylene glycol (EG) solution, 1.99g of an ethylene glycol antimony catalyst, and 1010g of an antioxidant were added. 3.01g, a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, the temperature was gradually raised, a pre-polycondensation reaction was carried out under the conditions of an absolute pressure of 0.1-100kPa for 45min, and a final polycondensation reaction was carried out under the conditions of a temperature of 284°C and an absolute pressure of 0.01-0.5kPa. After the stirring current of the reactor reached the set value, the final polycondensation time was 110min to obtain a melt, the melt was extruded through a melt pump, pelletized and dried to obtain 6011.1g of functional polyester.
[0108] Comparative Example 3
[0109] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 241g of isophthalic acid (IPA), 3000g of ethylene glycol (EG), 1.99g of ethylene glycol antimony catalyst and 3.01g of antioxidant 1010 were added, and the esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the esterification reaction, the acid value of the esterified product was tested to be 38mg. The invention discloses a method for preparing a functional polyester comprising the steps of: adding 310 g of a polyethylene glycol (PEG2000) / ethylene glycol (EG) solution having a polyethylene glycol concentration of 50 wt %, directly and gradually raising the temperature at 260° C., carrying out a pre-polycondensation reaction at an absolute pressure of 0.1-100 kPa for 45 min, carrying out a final polycondensation reaction at a temperature of 284° C. and an absolute pressure of 0.01-0.5 kPa, and waiting for the stirring current of the reactor to reach the set value and the final polycondensation time to be 98 min to obtain a melt; extruding the melt through a melt pump, pelletizing and drying the melt to obtain 6011.1 g of a functional polyester.
[0110] Comparative Example 4
[0111] The functional polyester was prepared according to the method of Example 1, except that the amount of ethylene glycol antimony catalyst was replaced by 1.73 g, the temperature of the final polycondensation reaction was replaced by 289° C., and the final polycondensation time was 130 min.
[0112] Comparative Example 5
[0113] The functional polyester was prepared according to the method of Example 4, except that polyethylene glycol PEG2000 was replaced by PEG800, and the final polycondensation reaction time was 100 min.
[0114] Comparative Example 6
[0115] The functional polyester was prepared according to the method of Example 4, except that polyethylene glycol PEG2000 was replaced by PEG6000, and the final polycondensation reaction time was 126 min.
[0116] Comparative Example 7
[0117] In a 20L general polymerization reactor, 4800g of terephthalic acid (PTA), 57g of isophthalic acid (IPA), 3100g of ethylene glycol (EG), 1.88g of ethylene glycol antimony catalyst and 2.84g of antioxidant 1010 were added, and the first stage of esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. At the end of the first stage of esterification reaction, the acid value of the esterified product was tested to be 38mg. The reaction kettle was cooled, and 114 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was added, and the second esterification reaction was continued at a temperature of 230°C for 40 min; after the second esterification reaction was completed, the temperature was gradually increased, and a pre-polycondensation reaction was carried out at an absolute pressure of 0.1-100 kPa for 45 min, and a final polycondensation reaction was carried out at a temperature of 284°C and an absolute pressure of 0.01-0.5 kPa. After the stirring current of the reaction kettle reached the set value, the final polycondensation time was 105 min to obtain a melt, and the melt was extruded through a melt pump, pelletized, and dried to obtain 5674.7 g of functional polyester.
[0118] Comparative Example 8
[0119] Functional polyester was prepared according to the method of Example 1, except that the acid value of the esterified product was controlled to 80 mg KOH / g at the end of the first stage esterification reaction. As a result, a large amount of PEG was extracted by the vacuum system during the pre-polycondensation reaction, blocking the vacuum system and failing to complete the polycondensation reaction.
[0120] Comparative Example 9
[0121] The functional polyester was prepared according to the method of Example 1, except that the acid value of the esterified product at the end of the first stage esterification reaction was controlled to 15 mg KOH / g, and the final polycondensation time was 120 min.
[0122] Comparative Example 10
[0123] The functional polyester was prepared according to the method of Example 1, except that 361 g of polyethylene glycol (PEG2000) / ethylene glycol (EG) solution with a polyethylene glycol concentration of 50 wt% was replaced by adding 180.5 g of ethylene glycol (EG) and mixing evenly, and then adding 180.5 g of polyethylene glycol (PEG2000), and the final polycondensation time was 112 min.
[0124] Test Example 1
[0125] The functional polyesters prepared in Example 1 to Example 10 and Comparative Example 1 to Comparative Example 10 were used as samples, the IPA content (weight %) and PEG content (weight %) in each sample were calculated, and the intrinsic viscosity, glass transition temperature Tg, diethylene glycol content (weight %) and b value of each sample were tested. The results are shown in Table 1.
[0126] Table 1
[0127]
[0128] Test Example 2
[0129] After drying the functional polyesters prepared in Examples 1 to 10 and Comparative Examples 1 to 10, fiber precursors were prepared using pilot spinning devices at a spinning temperature of 288°C and a spinning speed of 3000 m / min. The obtained fiber precursors were drawn to obtain drawn yarns at a drawing speed of 450 m / min and a drawing ratio of 1.85. The moisture regain of the drawn yarns was tested, and the results are shown in Table 2. The drawn yarns were woven into stockings and 3 wt % disperse blue dye was added at a bath ratio of 1:30 and a temperature of 100°C for 60 min. The dyeing rate and K / S value of the stockings after dyeing were tested, and the results are shown in Table 2.
[0130] Table 2
[0131] serial number Fiber moisture regain% Garter dyeing rate % Garter K / S value Remark Example 1 0.53 94.2 26.8 Example 2 0.55 95.7 28.5 Example 3 0.49 94.7 26.1 Example 4 0.56 94.8 28.0 Example 5 0.54 94.6 27.4 Example 6 0.51 95.2 26.4 Example 7 0.53 94.4 26.9 Many fiber breakages and defects Example 8 0.53 94.2 26.8 Many fiber breakages and defects Example 9 0.53 94.5 26.7 Many fiber breakages and defects Example 10 0.69 96.1 28.7 Fiber bonding and drawing Comparative Example 1 0.38 86.6 20.7 Comparative Example 2 / / / Comparative Example 3 0.49 91.7 23.4 Many fiber breakages and defects Comparative Example 4 0.42 93.7 23.9 Many fiber breakages and defects Comparative Example 5 0.44 90.7 22.4 Many fiber breakages and defects Comparative Example 6 0.45 92.4 23.7 Poor fiber operation Comparative Example 7 0.39 87.2 21.8 Comparative Example 8 / / / Comparative Example 9 0.48 92.8 25.1 Comparative Example 10 0.48 93.2 24.8
[0132] From the results of Table 1 and Table 2, it can be seen that in Examples 1 to 10, the functional polyester obtained by the preparation method provided by the present invention is introduced into the third monomer and the fourth monomer with a specific content and molecular chain length under the binary reaction system of terephthalic acid and ethylene glycol to achieve the regulation of the molecular structure of the polyester, and the preparation process is adjusted by segmented esterification, optimizing the addition method of the four monomers, and increasing the polymerization temperature to shorten the reaction time. The functional copolyester is prepared by the comprehensive effect of molecular structure regulation and process innovation. Compared with Examples 1 to 10, Comparative Examples 1 to 10 have problems such as slow polymerization reaction, abnormal polyester product indicators, unstable fiber processing and molding process, low fiber dyeing rate or insufficient actual monomer addition.
[0133] Compared with the conventional polyester in Comparative Example 1, the functional copolyester prepared in each embodiment of the present invention has an intrinsic viscosity of 0.50-0.69 dL / g and a glass transition temperature of 60°C-73°C, avoiding abnormal phenomena such as twisting and adhesion during the fiber forming process caused by the glass transition temperature, and has good processability. The moisture regain of the fiber prepared by the functional polyester provided by Examples 1 to 10 of the present invention is more than 34% higher than that of conventional polyester, indicating a significant hydrophilic effect; and the dyeing performance of the socks prepared by the functional polyester is significantly improved, and the dyeing rate is more than 8% higher than that of conventional polyester under the same dyeing process conditions, and the K / S value is more than 25% higher, and the dyeing performance is significantly improved.
[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A functional polyester fiber, It is characterized in that The dyeing rate of the functional polyester fiber is greater than 94%, and the K / S value is greater than 26.
2. The functional polyester fiber according to claim 1, It is characterized in that The moisture regain of the functional polyester fiber is 0.49-0.56%.
3. A method for preparing a functional polyester, It is characterized in that The steps include: (1) mixing an aromatic dibasic acid, ethylene glycol and a catalyst to carry out a contact reaction I; (2) subjecting the product obtained from the contact reaction I to a contact reaction II with a polyethylene glycol-ethylene glycol solution.
4. The preparation method according to claim 3, It is characterized in that The aromatic dibasic acid comprises a first aromatic dibasic acid and a second aromatic dibasic acid, and the catalyst is an antimony catalyst; Preferably, the first aromatic dibasic acid is terephthalic acid; the second aromatic dibasic acid is selected from at least one of isophthalic acid, 2,6-naphthalene dicarboxylic acid and 4,4'-biphenyl dicarboxylic acid, more preferably isophthalic acid; the antimony catalyst is selected from at least one of ethylene glycol antimony, antimony trioxide and antimony acetate; Preferably, the weight ratio of the first aromatic dibasic acid, the second aromatic dibasic acid, the ethylene glycol and the polyethylene glycol-ethylene glycol solution is 1:0.05-0.10:0.59-0.65:0.06-0.13; Preferably, the concentration of polyethylene glycol in the polyethylene glycol-ethylene glycol solution is 30-50% by weight; Preferably, the number average molecular weight of the polyethylene glycol is 1000-5000, more preferably 2000.
5. The preparation method according to claim 3 or 4, It is characterized in that In step (1), the conditions of the contact reaction I include at least: a temperature of 245-265° C. and a relative pressure of 0.24-0.26 MPa; the conditions for the termination of the contact reaction I include at least: an acid value of a product of the contact reaction I of 20-60 mg KOH / g.
6. The preparation method according to claim 3 or 4, It is characterized in that In step (2), the process of the contact reaction II includes: subjecting the product obtained from the contact reaction I to an esterification reaction and a polycondensation reaction with a polyethylene glycol-ethylene glycol solution; Preferably, the conditions of the esterification reaction include at least: temperature of 225-240°C, relative pressure of 0.24-0.26MPa, and time of 20-60min; Preferably, the polycondensation reaction process comprises: subjecting the product of the esterification reaction to a preliminary polycondensation reaction to obtain a prepolymerization product, and subjecting the prepolymerization product to a final polycondensation reaction; Preferably, the conditions of the pre-polycondensation reaction include at least: an absolute pressure of 0.1-100 kPa; Preferably, the conditions for the final polycondensation reaction include at least: a temperature of 282-286° C. and an absolute pressure of 0.01-0.5 kPa; and the conditions for the end of the final polycondensation reaction process include at least: a stirring current reaches a preset value.
7. The preparation method according to claim 3 or 4, It is characterized in that The method further comprises: adding an auxiliary agent during the contact reaction I; Preferably, the auxiliary agent is an antioxidant, more preferably a phenolic antioxidant; Preferably, the weight ratio of the auxiliary agent to the aromatic dibasic acid is 1:1650-1700.
8. The functional polyester obtained by the preparation method according to any one of claims 3 to 7; Preferably, the functional copolyester has an intrinsic viscosity of 0.50-0.69 dL / g and a glass transition temperature of 60°C-73°C.
9. A functional polyester fiber, It is characterized in that The functional polyester according to claim 8 is used for spinning.
10. Use of the functional polyester fiber according to claim 1, 2 or 8 and / or the functional polyester fiber according to claim 9 in the preparation of clothing products.