Preparation method of VDC-AN composition

Through the optimization of emulsion polymerization process and copolymerized emulsifier, the safety and operation complexity of organic solvents in the manufacturing of nitrile chlorine fibers are solved, and the preparation of green and environmentally friendly VDC-AN compositions is realized, which improves the flexibility of the fibers and Dyeing performance, suitable for flame retardant applications.

CN118955787AActive Publication Date: 2024-11-15ZHEJIANG QUZHOU JUSU CHEM IND CO LTD +1

Patent Information

Application Number
CN202410988645.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The use of organic solvents in the existing manufacturing methods of nitrile fibers leads to the risk of ignition, is not environmentally friendly and has cumbersome operation, and the emulsion method may leave emulsifier residues after demulsification, which affects the continuous operation of the device and increases costs.

Method used

By adopting the emulsion polymerization process, by optimizing the polymerization process, reaction temperature and time, introducing copolymerized emulsifiers and carboxylic acid or sulfonic acid groups, reducing the amount of emulsifier, realizing the preparation of VDC-AN compositions without washing process, and improving the spinning after Flexibility and dyeing properties of fibers.

Benefits of technology

The green and environmentally friendly preparation of VDC-AN composition is realized, the washing process is reduced, the flexibility and dyeing performance of the fiber are improved, and it is suitable for flame retardant clothing and fire-proof fields. The fiber performance is excellent after spinning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955787A_ABST
    Figure CN118955787A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a VDC-AN composition. The preparation method comprises the following steps: (1) preparing reaction raw materials for later use; (2) preparing an emulsifier aqueous solution; (3) preparing a polymerization initiator aqueous solution; (4) preparing an aqueous solution of a residue elimination initiator; (5) seed emulsion polymerization; (6) feeding and polymerizing; and (7) post-treatment. The method has the advantages of simple process, environmental protection, good product performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a VDC-AN composition. Background Art

[0002] Acrylic fiber (VDC-AN composite) is also called modified acrylic fiber, which is mainly obtained by polymerization of acrylonitrile (AN), vinylidene chloride (VDC), chromogens, etc. Compared with polyester fiber, acrylic fiber has the softness of natural fiber, excellent water absorption and good comfort, good dyeing performance and excellent fire retardant performance, and is favored by the high-end fiber market. Therefore, many technical experts in the industry are exploring the manufacturing method of acrylic fiber resin.

[0003] For example, CN104558392A discloses a method for manufacturing highly flame-retardant modified polyacrylonitrile and flame-retardant fiber, the manufacturing method comprising prepolymerizing a component A and a component B respectively to obtain a first prepolymer solution and a second prepolymer solution, and then blending or copolymerizing the first prepolymer solution and the second prepolymer solution in a predetermined ratio to obtain highly flame-retardant modified polyacrylonitrile with a molecular weight not greater than 80,000. Although the invention improves the dyeing, flame retardancy and processing properties of highly flame-retardant modified acrylonitrile fiber, it uses an organic solvent as a dispersion medium, and the organic solvent needs to be separated and purified later, is easy to catch fire during polymerization and operation, and is not green and environmentally friendly. In addition, two polymers need to be synthesized and then mixed, which is too cumbersome to operate.

[0004] For example, CN107734988A discloses acrylic fibers for artificial hair, a method for producing the same, and a headdress product comprising the same. The invention relates to an acrylic fiber for artificial hair, which is an acrylic fiber for artificial hair composed of an acrylic copolymer obtained by copolymerizing acrylonitrile, vinyl chloride and / or vinylidene chloride with a vinyl monomer containing a sulfonic acid group. The acrylic fiber for artificial hair contains 0.1 to 3% by mass of an organic solvent capable of dissolving the acrylic copolymer relative to the total mass of the acrylic fiber for artificial hair. The acrylic fiber for artificial hair has an average surface roughness of 5900 μm in a region of 40 μm in length and 80 μm in width on the side of the fiber. 2The following. The acrylic fiber for artificial hair of the present invention can be produced by wet spinning a spinning solution containing 8 to 16 parts by weight of water relative to 100 parts by weight of the above-mentioned acrylic copolymer. The present invention proposes to synthesize AN-VDC resin by emulsion method, and using sulfonate as initiator can well solve the problem of phase separation between chromogen (hydrophilic) and main monomers AN and VDC (lipophilic), and better solve the problem of dyeing nylon fiber. However, a part of anionic emulsifier is used, and there will be emulsifier residue in AN-VDC resin after demulsification in the later stage, which will increase the washing process, affect the continuous operation of the device and increase the cost. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a method for preparing a VDC-AN composition with simple process, environmental protection and good product performance.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a method for preparing a VDC-AN composition, comprising the following steps:

[0007] (1) Prepare reaction raw materials

[0008] By weight, the reaction raw materials consist of:

[0009]

[0010] (2) preparing an emulsifier aqueous solution: preparing an emulsifier aqueous solution by mixing a copolymerized emulsifier with 3-10% deionized water for later use;

[0011] (3) preparing a polymerization initiator aqueous solution: preparing a polymerization initiator aqueous solution by mixing 15-20% of an initiator with 10-20% of deionized water for later use;

[0012] (4) preparing a residual initiator aqueous solution: preparing a residual initiator aqueous solution by mixing the remaining initiator with 5-10% deionized water for later use;

[0013] (5) Seed emulsion polymerization: add the remaining deionized water, 5-10% of vinylidene chloride monomer, 5-10% of acrylonitrile monomer, 5-10% of chromogen, 5-10% of acrylate monomer, 5-10% of emulsifier aqueous solution to a polymerization kettle, cold disperse for 15-35 minutes at a stirring speed of 80-150 rpm, heat to 45-75° C., add 5-10% of polymerization initiator aqueous solution to react for 0.5-2.5 hours to obtain a seed emulsion;

[0014] (6) Adding polymerization: adding the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining chromogen, the remaining acrylate monomer, the remaining emulsifier aqueous solution, and the remaining polymerization initiator aqueous solution to the above seed emulsion at a temperature of 45 to 75° C. and a stirring speed of 80 to 150 rpm to react for 4 to 8 hours to obtain a reaction product;

[0015] (7) Post-treatment: adding an aqueous solution of a residual initiator to the reaction product obtained in step (6) at a temperature of 45 to 75° C. and a stirring speed of 80 to 150 rpm to carry out a reaction for 0.5 to 1.5 h. After the reaction is completed, the temperature is lowered and the material is discharged. The obtained material is demulsified, flash evaporated, and dried to obtain a VDC-AN composite.

[0016] As a preferred embodiment of the present invention, the polymerization kettle is evacuated before the seed emulsion polymerization.

[0017] As a preferred embodiment of the present invention, the chromatid is at least one of allyl sulfonic acid, methacrylic acid, isoprene sulfonic acid, 2-acrylamide-2-methylpropane sulfonic acid and metal salts and amine salts thereof.

[0018] As a preferred embodiment of the present invention, the acrylic acid ester monomer is at least one of methyl acrylate, n-butyl acrylate and isooctyl acrylate.

[0019] As a preferred embodiment of the present invention, the copolymeric emulsifier is at least one of dialkyl sulfosuccinic acid containing a double bond group, alkyl alcohol ether sulfuric acid containing a double bond group, allyl polyether phosphate, and metal salts and amine salts thereof.

[0020] As a preferred embodiment of the present invention, the structural formula of the dialkyl sulfosuccinic acid containing a double bond group is as follows:

[0021]

[0022] Among them, R1 is C6~C 14 A straight chain or branched alkane group, R2 is C6~C 14 R3 is an H group or a C1~C3 straight chain or branched alkane group.

[0023] The double bond-containing bis-alkyl sulfosuccinic acid is more preferably at least one of allyl didodecyl sulfosuccinic acid, allyl didoctyl sulfosuccinic acid and allyl didecyl sulfosuccinic acid.

[0024] As a preferred embodiment of the present invention, the structural formula of the alkyl alcohol ether sulfuric acid containing a double bond group is as follows:

[0025]

[0026] Among them, the range of a is 2 to 10, and the range of b is 2 to 8.

[0027] The double bond-containing alkyl alcohol ether sulfuric acid is more preferably at least one of allyl dodecyl alcohol ether sulfuric acid and allyl decanyl alcohol ether sulfuric acid.

[0028] As a preferred embodiment of the present invention, the structural formula of the allyl polyether phosphate is as follows:

[0029]

[0030] The range of n is 2 to 12.

[0031] The allyl polyether phosphate is more preferably allyl polyether (n=5) phosphate.

[0032] As a preferred embodiment of the present invention, the initiator is at least one of tert-butyl hydroperoxide and Rongalite.

[0033] As a preferred embodiment of the present invention, the flash evaporation temperature in step (7) is 60 to 80°C and the pressure is -0.09 to -0.01 MPa; the drying temperature is 35 to 70°C.

[0034] The preparation method of the VDC-AN composition of the present invention optimizes the preparation process by adopting the emulsion polymerization process and optimizing the factors affecting the reaction such as the polymerization process, reaction temperature and time, feeding formula, feeding method, etc., and well solves the problem of large differences in the reactivity rate of vinylidene chloride, acrylonitrile and chromogen, and obtains a VDC-AN composition with excellent copolymer structure. The present invention reduces the amount of emulsifier by introducing chromogen, effectively avoids the problem of residual auxiliary agent at the end of the reaction, reduces the washing process, and realizes the continuous production of the device. At the same time, by virtue of the excellent flexible groups and carboxylic acid or sulfonic acid groups of the copolymerized emulsifier, the VDC-AN composition obtained after spinning has better flexibility and dyeing performance. The VDC-AN composition obtained by the present invention is particularly suitable for spinning process, and can be widely used in flame-retardant clothing, flame-retardant furniture and many fire prevention fields.

[0035] In the present invention, latex particles of appropriate size are formed in the seed emulsion polymerization stage; in the feed polymerization stage, the monomers of the feed polymerization have a swelling effect on the latex particles formed in the previous seed emulsion polymerization stage (polymerization and swelling are carried out simultaneously). The introduction of the copolymeric emulsifier can ensure the stability of the latex ions while its special flexible structure can also effectively improve the fiber flexibility after spinning processing. At the same time, its shared carboxyl or sulfonic acid group also has good dyeing properties, achieving better dyeing properties of the fiber. The final composition does not need to be washed after mechanical demulsification. After flash evaporation to remove residual additives and water, it can enter the fluidized bed for drying to obtain a highly flame-retardant acrylic resin.

[0036] Compared with the prior art, the present invention has the following advantages:

[0037] 1. The present invention adopts an emulsion polymerization process, optimizes the factors affecting the reaction such as the polymerization process, reaction temperature and time, feed formula, and feed method, optimizes the preparation process, and effectively solves the problem of large differences in the reactivity rates of vinylidene chloride, acrylonitrile, and chromatin monomers. The obtained composition has better fiber uniformity after spinning, and the dyeing effect is more uniform, and there will be no phenomenon of different shades of color after dyeing.

[0038] 2. The present invention introduces a copolymer emulsifier, which ensures the stability of latex ions while its special flexible structure can effectively improve the fiber flexibility after spinning processing. At the same time, its shared carboxyl or sulfonic acid group also has good dyeing properties, achieving better dyeing properties of the fiber.

[0039] 3. The composition prepared by the present invention does not need to be washed after mechanical demulsification, and can be dried to obtain a VDC-AN composition after removing residual additives and water by flash evaporation.

[0040] 4. The fiber obtained by spinning the composition prepared by the present invention has excellent performance. The present invention introduces specific flexible and dyeing groups by introducing copolymeric emulsifiers, reduces the amount of flexible monomers and dyeing monomers, and further improves the fiber performance. The obtained fiber strength can reach more than 2.7 cN / dtex, the limiting oxygen index (LOI) can reach more than 31, and the coloring rate can reach more than 91%. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is the SEM picture of the resin of Example 4 of the present invention and Comparative Example 1.

[0042] Figure 2 It is the SEM picture of the fiber of Example 6 of the present invention and Comparative Example 2.

[0043] Among them, a1 and a2 are the morphologies of the resin state at different scales after demulsification in Example 4, b1 and b2 are the morphologies of the resin state at different scales in Comparative Example 1; a3 and a4 are the morphologies of the fiber state at different scales after spinning in Example 6, and b3 and b4 are the morphologies of the fiber state at different scales in Comparative Example 2. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below in conjunction with examples, but the present invention is not limited to the following examples.

[0045] Example 1

[0046] A method for preparing a VDC-AN composition comprises the following steps:

[0047] (1) Prepare reaction raw materials

[0048] The raw material formula is as follows:

[0049]

[0050] Polymerization initiator:

[0051] Tert-butyl hydroperoxide (TBHP) 30g

[0052] SFS 30g

[0053] Residue initiator:

[0054] Tert-butyl hydroperoxide 150g

[0055] 150g of Rongbai powder

[0056] Deionized water 70kg

[0057] (2) preparing an emulsifier aqueous solution: weigh 0.25 kg of allyl didodecyl sulfosuccinic acid and add 3 kg of deionized water to prepare an emulsifier aqueous solution for later use;

[0058] (3) Preparation of polymerization initiator aqueous solution: weigh 30 g of TBHP, add 5 kg of deionized water to prepare TBHP aqueous solution, and set aside; weigh 30 g of SFS, add 5 kg of deionized water to prepare SFS aqueous solution, and set aside;

[0059] (4) Preparation of aqueous solution of residual initiator: Weigh 150 g of TBHP and prepare a TBHP aqueous solution with 2 kg of deionized water for later use; weigh 150 g of SFS and prepare a SFS aqueous solution with 2 kg of deionized water for later use;

[0060] (5) Seed emulsion polymerization: first, add the remaining deionized water into a polymerization kettle, evacuate the polymerization kettle to -0.095 MPa, and while maintaining the vacuum, use a pump to pump 1 kg of vinylidene chloride monomer, 1.5 kg of acrylonitrile monomer, 75 g of sodium allyl sulfonate, 25 g of methyl acrylate and 10% of the aqueous emulsifier solution prepared in step (2) into the polymerization kettle, and cold disperse at a stirring speed of 100 rpm for 20 minutes. Maintain the speed and heat to 50° C., then uniformly add 10% of the TBHP aqueous solution prepared in step (3) and 10% of the SFS aqueous solution prepared in step (3) within 1 hour to react for 1 hour to obtain a seed emulsion;

[0061] (6) Adding feed polymerization: maintaining the polymerization kettle temperature at 50° C. and the stirring speed at 100 rpm, adding the remaining emulsifier aqueous solution, the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining sodium allyl sulfonate, the remaining methyl acrylate, the remaining TBHP aqueous solution prepared in step (3) and the SFS aqueous solution to the seed emulsion obtained in step (5) to carry out reaction, and the reaction is terminated after 8 hours to obtain a reaction product;

[0062] (7) Post-treatment: The TBHP aqueous solution and the SFS aqueous solution prepared in step (4) were uniformly pumped into the polymerization kettle over 30 minutes while maintaining the polymerization kettle temperature at 50°C and the stirring speed at 100 rpm. After the addition, the temperature was lowered to 30°C for discharge. The obtained material was mechanically demulsified and then dried in a flash tank at a flash temperature of 60°C and a flash pressure of -0.07 MPa. After the flash was completed, the material was dried in a fluidized bed at a drying temperature of 45°C to obtain the product.

[0063] Example 2

[0064] A method for preparing a VDC-AN composition comprises the following steps:

[0065] (1) Prepare reaction raw materials

[0066] The raw material formula is as follows:

[0067]

[0068] Polymerization initiator:

[0069] Tert-butyl hydroperoxide 32g

[0070] 32g of Rongbai powder

[0071] Residue initiator:

[0072] Tert-butyl hydroperoxide 160g

[0073] 160g of Rongbai powder

[0074] Deionized water 75kg

[0075] (2) preparing an emulsifier aqueous solution: weigh 0.5 kg of sodium allyl dodecyl alcohol ether sulfate and add 3 kg of deionized water to prepare an emulsifier aqueous solution for later use;

[0076] (3) Preparation of polymerization initiator aqueous solution: Weigh 32 g of TBHP and add 5 kg of deionized water to prepare a TBHP aqueous solution for later use; weigh 32 g of SFS and add 5 kg of deionized water to prepare an SFS aqueous solution for later use;

[0077] (4) Preparation of aqueous solution of residual initiator: Weigh 160 g of TBHP and prepare a TBHP aqueous solution with 2 kg of deionized water for later use; weigh 160 g of SFS and prepare a SFS aqueous solution with 2 kg of deionized water for later use;

[0078] (5) Seed emulsion polymerization: first, the remaining deionized water is added to the polymerization kettle, and the polymerization kettle is evacuated to -0.095 MPa. While maintaining the vacuum degree, 0.75 kg of vinylidene chloride monomer, 0.5 kg of acrylonitrile monomer, 25 g of sodium 2-acrylamide-2-methylpropane sulfonate, 25 g of n-butyl acrylate and 5% of the aqueous emulsifier solution prepared in step (2) are pumped into the polymerization kettle, and the mixture is cold dispersed at a stirring speed of 80 rpm for 25 minutes. The temperature is raised to 55° C. while maintaining the speed, and then 5% of the TBHP aqueous solution prepared in step (3) and 5% of the SFS aqueous solution prepared in step (3) are uniformly added within 1 hour to react for 1.5 hours to obtain a seed emulsion;

[0079] (6) Adding polymerization: maintaining the polymerization kettle temperature at 55° C. and the stirring speed at 80 rpm, adding the remaining emulsifier aqueous solution, the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining sodium 2-acrylamide-2-methylpropane sulfonate, the remaining n-butyl acrylate, the remaining TBHP aqueous solution prepared in step (3) and the SFS aqueous solution to the seed emulsion obtained in step (5) for reaction, and ending the reaction after 4 hours to obtain a reaction product;

[0080] (7) Post-treatment: The TBHP aqueous solution and the SFS aqueous solution prepared in step (4) were uniformly pumped into the polymerization kettle over 60 minutes while maintaining the polymerization kettle temperature at 55°C and the stirring speed at 80 rpm. After the addition, the temperature was lowered to 30°C for discharge. The obtained material was mechanically demulsified and then dried in a flash tank at a flash temperature of 70°C and a flash pressure of -0.05 MPa. After the flash was completed, the product was dried in a fluidized bed at a drying temperature of 50°C to obtain the product.

[0081] Example 3

[0082] A method for preparing a VDC-AN composition comprises the following steps:

[0083] (1) Prepare reaction raw materials

[0084] The raw material formula is as follows:

[0085]

[0086] Polymerization initiator:

[0087] Tert-butyl hydroperoxide 35g

[0088] 35g of Rongbai powder

[0089] Residue initiator:

[0090] Tert-butyl hydroperoxide 175g

[0091] 175g of Rongbai powder

[0092] Deionized water 60kg

[0093] (2) preparing an emulsifier aqueous solution: weigh 0.75 kg of allyl polyether (n=5) phosphate ester and add 3 kg of deionized water to prepare an emulsifier aqueous solution for later use;

[0094] (3) Preparation of polymerization initiator aqueous solution: weigh 35 g of TBHP, add 5 kg of deionized water to prepare TBHP aqueous solution, and set aside; weigh 35 g of SFS, add 5 kg of deionized water to prepare SFS aqueous solution, and set aside;

[0095] (4) Preparation of aqueous solution of residual initiator: Weigh 175 g of TBHP and prepare a TBHP aqueous solution with 2 kg of deionized water for later use; weigh 175 g of SFS and prepare a SFS aqueous solution with 2 kg of deionized water for later use;

[0096] (5) Seed emulsion polymerization: first, the remaining deionized water is added to the polymerization kettle, and the polymerization kettle is evacuated to -0.095 MPa. While maintaining the vacuum degree, 1 kg of vinylidene chloride monomer, 1 kg of acrylonitrile monomer, 60 g of sodium 2-acrylamide-2-methylpropane sulfonate, 12 g of isooctyl acrylate and 8% of the aqueous emulsifier solution prepared in step (2) are pumped into the polymerization kettle, and the mixture is cold dispersed at a stirring speed of 120 rpm for 20 minutes. The temperature is raised to 60° C. while maintaining the speed, and then 8% of the TBHP aqueous solution prepared in step (3) and 8% of the SFS aqueous solution prepared in step (3) are uniformly added within 1 hour to react for 2 hours to obtain a seed emulsion;

[0097] (6) Addition polymerization: maintaining the polymerization kettle temperature at 60° C. and the stirring speed at 120 rpm, adding the remaining emulsifier aqueous solution, the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining sodium 2-acrylamide-2-methylpropane sulfonate, the remaining isooctyl acrylate, the remaining TBHP aqueous solution prepared in step (3) and the SFS aqueous solution to the seed emulsion obtained in step (5) for reaction, and ending the reaction after 6 hours to obtain a reaction product;

[0098] (7) Post-treatment: The TBHP aqueous solution and the SFS aqueous solution prepared in step (4) were uniformly pumped into the polymerization kettle over 30 minutes while maintaining the polymerization kettle temperature at 60° C. and the stirring speed at 120 rpm. After the addition, the temperature was lowered to 30° C. and the material was discharged. The obtained material was mechanically demulsified and then dried in a flash tank at a flash temperature of 65° C. and a flash pressure of -0.09 MPa. After the flash was completed, the material was dried in a fluidized bed at a drying temperature of 45° C. to obtain the product.

[0099] Example 4

[0100] A method for preparing a VDC-AN composition comprises the following steps:

[0101] (1) Prepare reaction raw materials

[0102] The raw material formula is as follows:

[0103]

[0104] Polymerization initiator:

[0105] Tert-butyl hydroperoxide 32g

[0106] 32g of Rongbai powder

[0107] Residue initiator:

[0108] Tert-butyl hydroperoxide 150g

[0109] 150g of Rongbai powder

[0110] Deionized water 72kg

[0111] (2) preparing an emulsifier aqueous solution: weigh 0.5 kg of allyl decyl alcohol ether sodium sulfate, add 5 kg of deionized water to prepare an emulsifier aqueous solution for later use;

[0112] (3) Preparation of polymerization initiator aqueous solution: Weigh 32 g of TBHP and add 5 kg of deionized water to prepare a TBHP aqueous solution for later use; weigh 32 g of SFS and add 5 kg of deionized water to prepare an SFS aqueous solution for later use;

[0113] (4) Preparation of aqueous solution of residual initiator: Weigh 150 g of TBHP and prepare a TBHP aqueous solution with 2 kg of deionized water for later use; weigh 150 g of SFS and prepare a SFS aqueous solution with 2 kg of deionized water for later use;

[0114] (5) Seed emulsion polymerization: first, the remaining deionized water is added to the polymerization kettle, and the polymerization kettle is evacuated to -0.095 MPa. While maintaining the vacuum degree, 0.9 kg of vinylidene chloride monomer, 1.1 kg of acrylonitrile monomer, 20 g of sodium methyl propylene sulfonate, 20 g of sodium 2-acrylamide-2-methylpropane sulfonate, 40 g of methyl acrylate and 8% of the aqueous emulsifier solution prepared in step (2) are pumped into the polymerization kettle, and the mixture is cold dispersed at a stirring speed of 100 rpm for 20 minutes. The mixture is heated to 55° C. while maintaining the stirring speed. Then, 8% of the TBHP aqueous solution prepared in step (3) and 8% of the SFS aqueous solution prepared in step (3) are uniformly added within 1.5 hours to react for 1.5 hours to obtain a seed emulsion;

[0115] (6) Addition polymerization: maintaining the polymerization kettle temperature at 55° C. and the stirring speed at 100 rpm, adding the remaining emulsifier aqueous solution, the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining sodium methyl propylene sulfonate, the remaining sodium 2-acrylamide-2-methylpropane sulfonate, the remaining methyl acrylate, the remaining TBHP aqueous solution prepared in step (3) and the SFS aqueous solution to the seed emulsion obtained in step (5) for reaction, and ending the reaction after 6 hours to obtain a reaction product;

[0116] (7) Post-treatment: While maintaining the polymerization kettle temperature at 55° C. and the stirring speed at 100 rpm, the TBHP aqueous solution and the SFS aqueous solution prepared in step (4) were uniformly pumped into the polymerization kettle within 30 minutes. After the addition, the temperature was lowered to 30° C. and the material was discharged. After mechanical demulsification, the obtained material was placed in a flash tank for drying at a flash temperature of 70° C. and a flash pressure of -0.05 MPa. After the flash was completed, the material was placed in a fluidized bed for drying at a drying temperature of 50° C. to finally obtain the product.

[0117] Example 5

[0118] A method for preparing a VDC-AN composition comprises the following steps:

[0119] (1) Prepare reaction raw materials

[0120] The raw material formula is as follows:

[0121]

[0122] Polymerization initiator:

[0123] Tert-butyl hydroperoxide 34g

[0124] 34g of Rongbai powder

[0125] Residue initiator:

[0126] Tert-butyl hydroperoxide 170g

[0127] 170g of Rongbai powder

[0128] Deionized water 65kg

[0129] (2) preparing an emulsifier aqueous solution: weigh 0.75 kg of allyl bis-octyl sulfosuccinic acid and add 3 kg of deionized water to prepare an emulsifier aqueous solution for later use;

[0130] (3) Preparation of polymerization initiator aqueous solution: Weigh 34 g of TBHP and add 5 kg of deionized water to prepare a TBHP aqueous solution for later use; weigh 34 g of SFS and add 5 kg of deionized water to prepare an SFS aqueous solution for later use;

[0131] (4) Preparation of aqueous solution of residual initiator: Weigh 170 g of TBHP and prepare a TBHP aqueous solution with 2 kg of deionized water for later use; weigh 170 g of SFS and prepare a SFS aqueous solution with 2 kg of deionized water for later use;

[0132] (5) Seed emulsion polymerization: first, the remaining deionized water is added to the polymerization kettle, and the polymerization kettle is evacuated to -0.095 MPa. While maintaining the vacuum degree, 1.375 kg of vinylidene chloride monomer, 1.125 kg of acrylonitrile monomer, 25 g of isoprene sulfonic acid, 25 g of sodium allyl sulfonate, 25 g of methyl acrylate and 10% of the aqueous emulsifier solution prepared in step (2) are pumped into the polymerization kettle, and the mixture is cold dispersed at a stirring speed of 150 rpm for 15 minutes. The temperature is raised to 75° C. while maintaining the speed, and then 10% of the TBHP aqueous solution prepared in step (3) and 10% of the SFS aqueous solution prepared in step (3) are uniformly added within 1 hour for reaction. The reaction time is 1 hour to obtain a seed emulsion;

[0133] (6) Addition polymerization: maintaining the polymerization kettle temperature at 75° C. and the stirring speed at 150 rpm, adding the remaining emulsifier aqueous solution, the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining isoprene sulfonic acid, the remaining sodium allyl sulfonate, the remaining methyl acrylate, the remaining TBHP aqueous solution prepared in step (3) and the SFS aqueous solution to the seed emulsion obtained in step (5) for reaction, and ending the reaction after 4 hours to obtain a reaction product;

[0134] (7) Post-treatment: The TBHP aqueous solution and the SFS aqueous solution prepared in step (4) were uniformly pumped into the polymerization kettle over 90 minutes while maintaining the polymerization kettle temperature at 75°C and the stirring speed at 150 rpm. After the addition, the temperature was lowered to 30°C for discharge. The obtained material was mechanically demulsified and then dried in a flash tank at a flash temperature of 70°C and a flash pressure of -0.05 MPa. After the flash was completed, the product was dried in a fluidized bed at a drying temperature of 50°C to obtain the product.

[0135] Example 6

[0136] A method for preparing a VDC-AN composition comprises the following steps:

[0137] (1) Prepare reaction raw materials

[0138] The raw material formula is as follows:

[0139]

[0140] Polymerization initiator:

[0141] Tert-butyl hydroperoxide 30g

[0142] 30g of diatomite

[0143] Residue initiator:

[0144] Tert-butyl hydroperoxide 150g

[0145] 150g of Rongbai powder

[0146] Deionized water 70kg

[0147] (2) preparing an emulsifier aqueous solution: weigh 0.25 kg of allyl didecyl sodium sulfosuccinate and 0.25 kg of allyl dodecyl alcohol ether sodium sulfate, add 3 kg of deionized water to prepare an emulsifier aqueous solution for later use;

[0148] (3) Preparation of polymerization initiator aqueous solution: weigh 30 g of TBHP, add 5 kg of deionized water to prepare TBHP aqueous solution, and set aside; weigh 30 g of SFS, add 5 kg of deionized water to prepare SFS aqueous solution, and set aside;

[0149] (4) Preparation of aqueous solution of residual initiator: Weigh 150 g of TBHP and prepare a TBHP aqueous solution with 2 kg of deionized water for later use; weigh 150 g of SFS and prepare a SFS aqueous solution with 2 kg of deionized water for later use;

[0150] (5) Seed emulsion polymerization: first, add the remaining deionized water into a polymerization kettle, evacuate the polymerization kettle to -0.095 MPa, and while maintaining the vacuum, use a pump to pump 0.9 kg of vinylidene chloride monomer, 1.1 kg of acrylonitrile monomer, 20 g of sodium allyl sulfonate, 20 g of n-butyl acrylate and 8% of the aqueous emulsifier solution prepared in step (2) into the polymerization kettle, and cold disperse at a stirring speed of 100 rpm for 25 minutes. Maintain the speed and heat to 50° C., then uniformly add 8% of the TBHP aqueous solution prepared in step (3) and 8% of the SFS aqueous solution prepared in step (3) within 1 hour to react for 1.5 hours to obtain a seed emulsion;

[0151] (6) Adding feed polymerization: maintaining the polymerization kettle temperature at 50° C. and the stirring speed at 100 rpm, adding the remaining emulsifier aqueous solution, the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining sodium allyl sulfonate, the remaining n-butyl acrylate, the remaining TBHP aqueous solution prepared in step (3) and the SFS aqueous solution to the seed emulsion obtained in step (5) to carry out reaction, and the reaction is terminated after 6 hours to obtain a reaction product;

[0152] (7) Post-treatment: While maintaining the polymerization kettle temperature at 50° C. and the stirring speed at 100 rpm, the TBHP aqueous solution and the SFS aqueous solution prepared in step (4) were uniformly pumped into the polymerization kettle within 45 minutes. After the addition, the temperature was lowered to 30° C. for discharge. The obtained material was mechanically demulsified and then dried in a flash tank at a flash temperature of 70° C. and a flash pressure of -0.05 MPa. After the flash was completed, the material was dried in a fluidized bed at a drying temperature of 50° C. to finally obtain the product.

[0153] Comparative Example 1

[0154] A mixed solution of modified polyacrylonitrile was prepared according to the method described in Example 1 of CN104558392A.

[0155] Comparative Example 2

[0156] The acrylic copolymer latex was prepared according to the method described in Example 1 of CN107734988A.

[0157] Performance Testing

[0158] The compositions prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were used to prepare spun fibers, and the preparation process was as follows:

[0159] The composition was dissolved in dimethyl sulfoxide to prepare a resin solution having a resin concentration of 23.0 wt% (wt%, mass percentage concentration) and a water concentration of 2.0 wt%. The spinning solution was then extruded into a coagulation bath of a 65 mass% dimethyl sulfoxide aqueous solution at 20°C using a spinning nozzle and coagulated to form fibers, and then stretched and washed. The washed primary stretched yarn was then immersed in an oil tank into which a mixture of an oil and dimethyl sulfoxide was introduced, and finally dried at 120°C and stretched and relaxed to obtain VDC-AN fibers. The properties are shown in the following table, where:

[0160] Fiber strength test: carried out according to the method specified in GB / T 14337-2022 "Test method for tensile properties of chemical staple fibers";

[0161] Dyeing rate: according to the method specified in FZ / T 50024-2014 "Test method for dyeing rate of acrylic fiber";

[0162] Limiting oxygen index (LOI) test: carried out in accordance with the method specified in FZ / T 50029-2015 "Test method for flame retardancy of synthetic fiber raw material chips".

[0163]

[0164]

Claims

1. A method for preparing a VDC-AN composition, It is characterized in that The following steps are involved: (1) Prepare reaction raw materials By weight, the reaction raw materials consist of: (2) preparing an emulsifier aqueous solution: preparing an emulsifier aqueous solution by mixing a copolymerized emulsifier with 3-10% deionized water for later use; (3) preparing a polymerization initiator aqueous solution: preparing a polymerization initiator aqueous solution by mixing 15-20% of an initiator with 10-20% of deionized water for later use; (4) preparing a residual initiator aqueous solution: preparing a residual initiator aqueous solution by mixing the remaining initiator with 5-10% deionized water for later use; (5) Seed emulsion polymerization: add the remaining deionized water, 5-10% of vinylidene chloride monomer, 5-10% of acrylonitrile monomer, 5-10% of chromogen, 5-10% of acrylate monomer, 5-10% of emulsifier aqueous solution to a polymerization kettle, cold disperse for 15-35 minutes at a stirring speed of 80-150 rpm, heat to 45-75° C., add 5-10% of polymerization initiator aqueous solution to react for 0.5-2.5 hours to obtain a seed emulsion; (6) Adding polymerization: adding the remaining vinylidene chloride monomer, the remaining acrylonitrile monomer, the remaining chromogen, the remaining acrylate monomer, the remaining emulsifier aqueous solution, and the remaining polymerization initiator aqueous solution to the above seed emulsion at a temperature of 45 to 75° C. and a stirring speed of 80 to 150 rpm to react for 4 to 8 hours to obtain a reaction product; (7) Post-treatment: adding an aqueous solution of a residual initiator to the reaction product obtained in step (6) at a temperature of 45 to 75° C. and a stirring speed of 80 to 150 rpm to carry out a reaction for 0.5 to 1.5 h. After the reaction is completed, the temperature is lowered and the material is discharged. The obtained material is demulsified, flash evaporated, and dried to obtain a VDC-AN composite.

2. The method for preparing the VDC-AN composition according to claim 1, It is characterized in that The polymerization kettle is evacuated before the seed emulsion polymerization.

3. The method for preparing the VDC-AN composition according to claim 1, It is characterized in that The chromatid is at least one of allyl sulfonic acid, methacrylic acid, isoprene sulfonic acid, 2-acrylamide-2-methylpropane sulfonic acid and metal salts and amine salts thereof.

4. The method for preparing the VDC-AN composition according to claim 1, It is characterized in that The acrylic acid ester monomer is at least one of methyl acrylate, n-butyl acrylate and isooctyl acrylate.

5. The method for preparing the VDC-AN composition according to claim 1, It is characterized in that The copolymer emulsifier is at least one of dialkyl sulfosuccinic acid containing a double bond group, alkyl alcohol ether sulfuric acid containing a double bond group, allyl polyether phosphate, and metal salts and amine salts thereof.

6. The method for preparing the VDC-AN composition according to claim 5, It is characterized in that The structural formula of the dialkyl sulfosuccinic acid containing a double bond group is as follows: Among them, R 1 C 6 ~C 14 A straight chain or branched alkane group, R 2 C 6 ~C 14 A straight chain or branched alkane group, R 3 is H group or C 1 ~C 3 A straight chain or branched alkane group.

7. The method for preparing the VDC-AN composition according to claim 5, It is characterized in that The structural formula of the alkyl alcohol ether sulfuric acid containing a double bond group is as follows: Among them, the range of a is 2 to 10, and the range of b is 2 to 8.

8. The method for preparing the VDC-AN composition according to claim 5, It is characterized in that The structural formula of the allyl polyether phosphate is as follows: The range of n is 2 to 12.

9. The method for preparing the VDC-AN composition according to claim 1, It is characterized in that The initiator is at least one of tert-butyl hydroperoxide and Rongalite.

10. The method for preparing the VDC-AN composition according to claim 1, It is characterized in that The flash evaporation temperature in step (7) is 60-80°C and the pressure is -0.09-0.01Mpa; the drying temperature is 35-70°C.

Citation Information

Patent Citations

  • Method for synthesizing high-solubility copolymer resin of chloroethylene and acrylonitrile

    CN101608005A

  • Vinylidene chloride slow-release emulsion for oil recovery assistant and preparation method thereof

    CN107699211A

  • Acrylic fiber for artificial hair, method for manufacturing said fiber, and headdress product containing said fiber

    CN107734988A

  • Process for the production of modacrylic copolymers and acrylic copolymers thus obtained

    CN1119654A

  • Reactive emulsifier modified chlorinated polyether emulsion and preparation method thereof

    CN112552445A

Cited By

  • VDC-an composition and preparation method therefor

    WO2026020780A1