Preparation method of high-stability and high-adsorption MOF nanofiber membrane

The MOF nanofiber membrane prepared by electrospinning and coordination-induced self-assembly technology solves the problems of insufficient stability and easy dissolution of MOF in water, achieves high adsorption performance and water stability, and is suitable for efficient water treatment.

CN118895609APending Publication Date: 2024-11-05JIANGSU OCEAN UNIV

Patent Information

Application Number
CN202410995411.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The problems of existing MOF materials in water media are insufficient, the difficulty of powder separation from water and easy dissolution are limited, which limit their application in the field of water treatment.

Method used

Electrospinning method and coordination-induced self-assembly method are used to prepare high-stable, highly adsorbed MOF nanofiber membranes. Through nanofibers, the coordination bond strength is enhanced and adsorption sites are provided.

Benefits of technology

It has achieved the improvement of water stability and adsorption performance of MOF, solved the problems of easy shedding and high dissolution rate of MOF, and provided efficient water treatment adsorption materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895609A_ABST
    Figure CN118895609A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-stability and high-adsorption MOF (Metal Organic Framework) nanofiber membrane, and particularly relates to a preparation method of a high-stability Cu-BTC (Carboxymethyl Chitosan) (CMC) / PVDF (Polyvinylidene Fluoride) nanofiber membrane. The preparation method specifically comprises the following steps: firstly, preparing a spinning solution of a metal salt / fiber-forming polymer for synthesizing MOF, and uniformly dispersing metal ions in a nanofiber membrane through an electrostatic spinning method; and then inversely soaking the MOF nanofiber membrane in a solution of a ligand and a coordination polymer for synthesizing MOF, and carrying out coordination-induced self-assembly to obtain the MOF nanofiber membrane. The coordination polymer is self-assembled into the MOF structure, so that the strength of an MOF coordination bond is increased, the stability of the MOF structure is effectively improved, a molecular chain segment of the coordination polymer contains a large number of coordination functional groups (-NH,-COOH and the like), a large number of adsorption sites can be provided, and the MOF nanofiber membrane with high stability and high adsorption is constructed through coordination-induced self-assembly synergistically.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nanofiber membrane preparation and adsorption application, and specifically relates to a method for preparing a highly stable and highly adsorbing MOF nanofiber membrane. Background Art

[0002] With the rapid growth of the global population, the acceleration of urbanization and industrialization, the problem of water pollution is becoming increasingly serious. If wastewater is discharged directly without proper treatment, it will cause serious damage to the water body. Taking the textile industry as an example, the large amount of dye wastewater it produces contains organic dyes and heavy metal ions, almost all of which are toxic. In particular, the complexity of the molecular structure of dyes makes them difficult to decompose in water, highly stable to light, and resistant to biodegradation. To date, a variety of technologies have been developed to treat industrial wastewater. Among them, the adsorption method is considered to be one of the simplest and most efficient solutions for treating industrial wastewater because it can effectively remove pollutants such as suspended particles, organic matter and metal ions in water, and has the characteristics of simple process, easy management and operation.

[0003] Metal-organic framework (MOF) is a new type of porous organic-inorganic hybrid material with large porosity and specific surface area, showing great application potential in the fields of adsorption separation and wastewater treatment. However, some MOF materials, such as Cu-BTC, have relatively weak metal coordination bonds, resulting in insufficient stability of their skeletons in aqueous media. Coordination polymers containing coordination functional groups such as -COOH and -NH in the molecular chain segments are self-assembled on MOFs. The coordination polymers increase the strength of the coordination bonds and effectively increase the adsorption sites, which is expected to achieve a simultaneous improvement in the water stability and adsorption performance of MOFs.

[0004] In addition, MOF powders are widely used in water treatment due to their insolubility, poor processability, brittleness, and difficulty in separation from aqueous solutions. In order to solve this problem, MOF is combined with nanofiber carriers with high porosity and high specific surface area, which not only achieves innovative breakthroughs in morphology, structure and chemical properties, but also brings opportunities for the advancement of more efficient water treatment technology. However, MOF nanofiber materials prepared by the existing blending method generally have the disadvantages of poor bonding between MOF and polymer materials, easy detachment of MOF, and poor dispersibility of MOF.

[0005] In view of the above shortcomings, the development of a method for preparing MOF nanofiber membranes that is water-stable, highly adsorbable, not easily dissolved, and simple and easy is the focus of current research. Summary of the invention

[0006] The purpose of the present invention is to address the problems of insufficient stability of MOF in water, difficulty in separating MOF powder from aqueous media and easy dissolution of MOF. It proposes a method of using electrospinning and coordination-induced self-assembly to in situ prepare highly stable and highly adsorbable MOF from the surface of the fiber membrane, construct a MOF nanofiber membrane with both water stability and high adsorption and separation performance, and provide a new adsorption material for efficient water treatment.

[0007] The technical solution of the present invention: The MOF nanofiber membrane is prepared by electrostatic spinning and coordination induced self-assembly, and is composed of MOF, coordination polymer, and nanofiber membrane. The nanofiber part runs through the MOF structure. The coordination polymer coordinates with the MOF metal site to enhance the coordination bond strength of MOF and provide effective adsorption sites.

[0008] The above-mentioned method for preparing a highly stable and highly adsorbable MOF nanofiber membrane specifically comprises the following steps: (1) A certain amount of metal salt and fiber-forming polymer for synthesizing MOF are dissolved in a solvent, heated and stirred to prepare a metal salt / fiber-forming polymer spinning solution, and a metal salt / fiber-forming polymer nanofiber membrane is prepared by electrospinning, which is denoted as M. n+ / fiber-forming polymer nanofiber membranes; The synthesized MOF includes but is not limited to one or more of Cu-BTC, MOF-5, ZIF-8, ZIF-67, and UiO-66, preferably Cu-BTC.

[0009] The metal salts used to synthesize MOF include but are not limited to Cu(NO3)2·3H2O, Zn(NO3)2·6(H2O), Co(NO3)2·6(H2O), ZrCl4, etc.

[0010] The fiber-forming polymer is a high molecular polymer that can be used to prepare nanofiber membranes by electrospinning, including but not limited to one or more of polytetrafluoroethylene (PVDF), polyacrylonitrile (PAN), and polysulfone (PSf), preferably PVDF.

[0011] The solvent is a commonly used solvent in the art, including but not limited to one or more of N,N-dimethylformamide and acetone, ethanol, chloroform, dichloromethane, and acetic acid. For the preferred fiber-forming polymer PVDF, the preferred solution is a mixture of N,N-dimethylformamide and acetone, with a mass ratio of 5:1 to 1:1.

[0012] The concentration of the metal salt in the metal salt / fiber-forming polymer spinning solution is 0.001 wt% to 3 wt%; the concentration of the fiber-forming polymer is 5 wt% to 20 wt%.

[0013] The electrospinning conditions are: voltage: 12-25 kV, spinning rate: 0.0005-0.3 mm / s, receiving distance: 5-20 cm.

[0014] In M n+ In the preparation process of polymer nanofiber membrane, the limitation of the above parameters is very important. Each link is closely linked and directly affects the M n+ / Metal ion distribution, fiber morphology and mechanical properties of fiber-forming polymer nanofiber membranes.

[0015] (2) Substitute the M obtained in step (1) n+ The fiber-forming polymer nanofiber membrane is inverted and immersed in a solution of a ligand and a coordination polymer for synthesizing MOF, and the MOF nanofiber membrane is obtained after the coordination-induced self-assembly reaction is sufficient.

[0016] The ligands used to synthesize MOF include but are not limited to trimesic acid, terephthalic acid, 2-methylimidazole, and the like.

[0017] The solvent is a commonly used solvent in the art, including but not limited to one or more of water, methanol, ethanol, n-butanol, ethyl acetate, and dichloromethane, and does not dissolve the fiber-forming polymer nanofiber membrane.

[0018] The coordination polymer contains coordination functional groups such as -COOH and -NH in the molecular chain segments, including but not limited to one or more of polyethyleneimine, polyvinylamine, chitosan, carboxymethyl chitosan, polyacrylic acid and amino acid, preferably carboxymethyl chitosan (CMC).

[0019] The molar ratio of the ligand to the coordination polymer is 100:1 to 1:1.

[0020] For the preferred fiber-forming polymers PVDF and MOF (Cu-BTC), step (1) is achieved by the following operations: 0.01~2g Cu(NO3)2·3H2O and 10~15g PVDF were dissolved in a mixed solvent of DMF and acetone with a mass ratio of 3:1, and heated and stirred at 60℃ for 8 hours to obtain Cu 2+ / PVDF spinning solution. The spinning solution was injected into the spinning needle tube, and electrospinning was performed under the spinning conditions of voltage: 12~20 kV, spinning rate: 0.0005~0.3 mm / s, and receiving distance: 5~20 cm to obtain Cu 2+ / PVDF nanofiber membrane.

[0021] For the preferred coordination polymer carboxymethyl chitosan (CMC), step (2) is achieved by the following operation: The Cu obtained in step (1) 2+The / PVDF nanofiber membrane is inverted and immersed in a mixed solution of ethanol and water with a molar ratio of 50:1~2:1 of trimesic acid and CMC. The volume ratio of ethanol: water is 1:0.01~1:1. After 12 hours of coordination-induced self-assembly reaction, it is taken out, washed and dried to obtain the Cu-BTC@CMC / PVDF nanofiber membrane. The following beneficial effects can be obtained by the above technical solution: The highly stable and highly adsorbable MOF nanofiber membrane of the present invention utilizes coordination polymers and MOF metal sites for self-assembly to enhance the coordination bond strength of MOF, thereby enhancing the water stability of MOF; at the same time, the pore structure of MOF and the coordination functional groups on the molecular chain segments of the coordination polymer provide effective adsorption sites.

[0022] In-situ preparation allows the nanofibers to partially penetrate the MOF structure, ensuring a low dissolution rate of MOF and solving the problem of easy MOF shedding. At the same time, it also solves the problem of poor mechanical properties of nanofibers in related technologies.

[0023] The present invention combines the advantages of large specific surface area of ​​polymer fiber membrane, excellent pore structure of MOF, adsorption performance of coordination polymer, etc., to synergistically construct a MOF nanofiber membrane with high stability and high adsorption.

[0024] The preparation method of the present invention has the advantages of simple process, easy large-scale preparation, etc., is suitable for industrial-scale production, and has certain universality. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is an optical image of the dye adsorption test of the Cu-BTC / PVDF nanofiber membrane in Example 1 at 25°C.

[0026] Figure 2 This is an optical image of the dye adsorption test of the Cu-BTC / PVDF nanofiber membrane in Example 1 at 80°C.

[0027] Figure 3 This is the optical image of the dye adsorption test of the Cu-BTC@CMC / PVDF nanofiber membrane in Example 2 at 80 °C. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below through several specific embodiments, but the present application is not limited thereto. Without departing from the content and scope of the present invention, any changes and implementations should be included in the technical scope of the present invention. Example 1

[0029] A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane, wherein the material is a Cu-BTC / PVDF nanofiber membrane, and the preparation steps are as follows: (1) 1.5 g of Cu(NO3)2·3H2O and 12 g of PVDF were dissolved in a mixed solvent of DMF and acetone in a mass ratio of 3:1, and heated and stirred at 60 °C for 8 hours to obtain Cu 2+ / PVDF spinning solution. The spinning solution was injected into a 5 mL spinning needle tube and electrospun under the spinning conditions of voltage 16 kV, spinning rate: 0.002 mm / s, and receiving distance: 12 cm to obtain Cu 2+ / PVDF nanofiber membrane.

[0030] (2) The Cu obtained in step (1) 2+ The Cu-BTC / PVDF nanofiber membrane was immersed upside down in 300 mL of a 1:1 ethanol / water mixed solution containing 1.26 g of trimesic acid. After 12 hours of coordination-induced self-assembly reaction, the membrane was taken out, washed and dried to obtain the Cu-BTC / PVDF nanofiber membrane.

[0031] A Congo red dye solution with a concentration of 100 ppm was prepared, and the Cu-BTC / PVDF nanofiber membrane in Example 1 was used as the adsorption membrane. The dye adsorption test was performed at 25°C and 80°C, respectively. The obtained optical images are shown in FIG. Figure 1 and Figure 2 shown.

[0032] Figure 1 This indicates that the dye adsorption capacity of Cu-BTC / PVDF nanofiber membrane is relatively low. Figure 2 This indicates that high temperature causes the structural collapse of the Cu-BTC skeleton and Cu-BTC is unstable in water. Example 2

[0033] A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane, wherein the material is Cu-BTC@carboxymethyl chitosan (CMC) / PVDF nanofiber membrane, and the preparation steps are as follows: (1) Dissolve a certain amount of Cu(NO3)2·3H2O and PVDF in a solvent, heat and stir to prepare Cu 2+ / PVDF spinning solution, Cu prepared by electrospinning 2+ / PVDF nanofiber membrane, the specific steps are the same as step (1) of Example 1.

[0034] (2) The Cu obtained in step (1) 2+ The Cu-BTC@CMC / PVDF nanofiber membrane was immersed upside down in a 300 mL 1:1 ethanol-water mixed solution containing 1.26 g trimesic acid and 0.126 g CMC. After 12 hours of coordination-induced self-assembly reaction, it was taken out, washed and dried to obtain the Cu-BTC@CMC / PVDF nanofiber membrane.

[0035] A Congo red dye solution with a concentration of 100 ppm was prepared, and the Cu-BTC@CMC / PVDF nanofiber membrane in Example 2 was used as the adsorption membrane. The dye adsorption test was carried out at 80 °C. The obtained optical image is shown in FIG. Figure 3 shown.

[0036] Figure 3 It shows that the addition of coordination polymer enhances the stability of Cu-BTC. Cu-BTC@CMC / PVDF nanofiber membrane has excellent adsorption performance. Example 3

[0037] A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane, wherein the material is Cu-BTC@polyethyleneimine (PEI) / PVDF nanofiber membrane, and the preparation steps are as follows: (1) Dissolve a certain amount of Cu(NO3)2·3H2O and PVDF in a solvent, heat and stir to prepare Cu 2+ / PVDF spinning solution, Cu prepared by electrospinning 2+ / PVDF nanofiber membrane, the specific steps are the same as step (1) of Example 1.

[0038] (2) The Cu obtained in step (1) 2+ The / PVDF nanofiber membrane is immersed upside down in a solution of a ligand and a coordination polymer for synthesizing MOF, and a MOF nanofiber membrane is obtained after the coordination-induced self-assembly reaction is sufficient. The specific steps are the same as step (2) of Example 2, except that the coordination polymer is PEI. Example 4

[0039] A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane, wherein the material is a ZIF-8@CMC / PVDF nanofiber membrane, and the preparation steps are as follows: (1) Dissolve a certain amount of Zn(NO3)2·6(H2O) and PVDF in a solvent, heat and stir to prepare Zn 2+ / PVDF spinning solution, electrospinning to obtain Zn 2+ / PVDF nanofiber membrane, the specific steps are the same as step (1) of Example 1.

[0040] (2) Zn obtained in step (1) 2+ The / PVDF nanofiber membrane is inverted and immersed in a solution of a ligand and a coordination polymer for synthesizing MOF, and a MOF nanofiber membrane is obtained after the coordination-induced self-assembly reaction is sufficient. The specific steps are the same as step (2) of Example 2, except that the ligand is 2-methylimidazole. Example 5

[0041] A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane, wherein the material is a UiO-66@CMC / PVDF nanofiber membrane, and the preparation steps are as follows: (1) Dissolve a certain amount of ZrCl4 and PVDF in a solvent, heat and stir to prepare Zr 4+ / PVDF spinning solution, electrospinning to obtain Zr 4+ / PVDF nanofiber membrane, the specific steps are the same as step (1) of Example 1.

[0042] (2) Zr obtained in step (1) 4+ The / PVDF / PVDF nanofiber membrane is immersed upside down in a solution of a ligand and a coordination polymer for synthesizing MOF, and a MOF nanofiber membrane is obtained after the coordination-induced self-assembly reaction is sufficient. The specific steps are the same as step (2) of Example 2, except that the ligand is terephthalic acid.

[0043] The above specific implementations are only a detailed explanation of the technical solutions of the present invention. The present invention is not limited to the above embodiments. Those skilled in the art should understand that any improvement or substitution based on the above principles and spirits on the basis of the present invention should be within the protection scope of the present invention. The above are all preferred implementations of the present invention. For those of ordinary skill in the art, without departing from the principle of the present invention, modifications to various equivalent forms of the present invention belong to the protection scope of the claims attached to this application.

Claims

1. A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane, characterized in that The specific steps include: A certain amount of metal salt and fiber-forming polymer for synthesizing MOF are dissolved in a solvent, heated and stirred to prepare a metal salt / fiber-forming polymer spinning solution, and a metal salt / fiber-forming polymer nanofiber membrane is prepared by electrospinning, which is denoted as M. n+ / fiber-forming polymer nanofiber membranes; The synthesized MOF includes but is not limited to one or more of Cu-BTC, MOF-5, ZIF-8, ZIF-67, and UiO-66; Among them, the metal salts used to synthesize MOF include but are not limited to one or more of Cu(NO3)2·3H2O, Zn(NO3)2·6(H2O), Co(NO3)2·6(H2O), and ZrCl4; The fiber-forming polymer is a high molecular polymer that can be used to prepare nanofiber membranes by electrospinning, including but not limited to one or more of polytetrafluoroethylene PVDF, polyacrylonitrile PAN, polysulfone PSf, and sulfonated polysulfone SPSf; The solvent used is a common solvent, including but not limited to one or more of N,N-dimethylformamide, acetone, ethanol, chloroform, dichloromethane, and acetic acid; The M obtained in step (1) n+ / Fiber-forming polymer nanofiber membrane is immersed upside down in a solution of ligand and coordination polymer for synthesizing MOF, and MOF nanofiber membrane is obtained after coordination-induced self-assembly reaction is sufficient; Among them, the ligands used to synthesize MOF include but are not limited to trimesic acid, terephthalic acid, and 2-methylimidazole; The solvent used is a common solvent, including but not limited to one or more of water, methanol, ethanol, n-butanol, ethyl acetate, and dichloromethane.

2. The method for preparing a highly stable and highly adsorbable MOF nanofiber membrane according to claim 1, characterized in that: In step (1), the concentration of the metal salt in the metal salt / fiber-forming polymer spinning solution is 0.001 wt% to 3 wt%; the concentration of the fiber-forming polymer is 5 wt% to 20 wt%.

3. The method for preparing a highly stable and highly adsorbable MOF nanofiber membrane according to claim 1, characterized in that: The electrospinning conditions in step (1) are: voltage: 12~25 kV; spinning rate: 0.0005~0.3 mm / s; receiving distance: 5~20 cm.

4. The method for preparing a highly stable and highly adsorbable MOF nanofiber membrane according to claim 1, characterized in that: The coordination polymer selected in step (2) contains coordination functional groups such as -COOH and -NH in the molecular chain segments, including but not limited to one or more of polyethyleneimine, polyvinylamine, chitosan, carboxymethyl chitosan, polyacrylic acid and amino acid.

5. The method for preparing a highly stable and highly adsorbable MOF nanofiber membrane according to claim 1, characterized in that: In step (2), the mass ratio of the ligand to the coordination polymer is 100:1~1:

1.

6. A method for preparing a highly stable and highly adsorbable MOF nanofiber membrane according to any one of claims 1 to 5, characterized in that For the preferred fiber-forming polymers PVDF and MOF (Cu-BTC), step (1) is achieved by the following operations: 0.01~2g Cu(NO3)2·3H2O and 10~15g PVDF were dissolved in a mixed solvent of DMF and acetone with a mass ratio of 3:1, and heated and stirred at 60℃ for 8 hours to obtain Cu 2+ / PVDF spinning solution; inject the spinning solution into the spinning needle tube, and perform electrospinning under the spinning conditions of voltage: 12~20 kV, spinning rate: 0.0005~0.3 mm / s, and receiving distance: 5~20 cm to obtain Cu 2+ / PVDF nanofiber membrane.

7. A method for preparing a highly stable and highly adsorbent MOF nanofiber membrane according to any one of claims 1 to 5, characterized in that For the preferred coordination polymer carboxymethyl chitosan CMC, step (2) is achieved by the following operation: The Cu obtained in step (1) 2+ The / PVDF nanofiber membrane was inverted and immersed in a mixed solution of ethanol and water with a mass ratio of 50:1~2:1 of trimesic acid and CMC; the volume ratio of ethanol: water was 1:0.01~1:

1. After 12 hours of coordination-induced self-assembly reaction, it was taken out, washed and dried to obtain the Cu-BTC@CMC / PVDF nanofiber membrane.

Citation Information

Patent Citations

  • Metal organic framework material and preparation method and application thereof

    CN106622139A

  • Ultra-low temperature metal organic ligand doped amino acid composite material and preparation method thereof

    CN107913676A

  • Carboxymethyl cellulose-zeolite imidazole skeleton-structural nano-sheet composite gas separation film as well as preparation method and application thereof

    CN108079799A

  • Preparation method for chitosan nanofiber membrane of in-situ growth of metal-organic frameworks

    CN108816064A

  • Adjustable-loading-form PAN / ZIF-67 composite material and preparation method thereof

    CN110578254A

Cited By

  • Flexible and high-strength composite piezoelectric fiber film as well as preparation method and application thereof

    CN119465512A

  • PVDF (Polyvinylidene Fluoride)-coated Zn3 (HHTP) 2 nano-fiber composite film for friction nano-generator and preparation method thereof

    CN119531043A

  • Cooperative refrigeration super-fabric based on polylactic acid oriented fibers and preparation method thereof

    CN120006447A