Antibacterial and antiviral artificial leather and preparation method thereof
By using the combination of antibacterial and antiviral agents containing activated zinc oxide, powder ammonia-resistant agents and ultraviolet absorbers in artificial leather, the problem of poor sterilization effect in vehicle applications is solved, and the car is achieved Effective sterilization and ammonia resistance improvement.
Patent Information
- Application Number
- CN202411181579.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-05
AI Technical Summary
The existing sterilization artificial leather containing activated zinc oxide is not used in the vehicle environment, and the specific surface area is insufficient for photon energy and insufficient specific surface area, resulting in poor sterilization effect and cannot be effectively used in practical applications.
Design an antibacterial and antiviral artificial leather, adopting a top-down stacked structure, including an antibacterial and antiviral agent containing activated zinc oxide, a powder ammonia-resistant agent and an ultraviolet absorber, and converts ultraviolet light into visible light through the ultraviolet absorber. Improve the light energy reception of activated zinc oxide and increase the specific surface area through powder ammonia-resistant agents, activated zinc oxide surface defects to generate O2- and OH-ions to attack bacteria and viruses.
It achieves effective bactericidal effect in the automotive environment, improves the ammonia resistance of artificial leather, and destroys the bacterial membrane structure through the activated zinc oxide, inhibits bacterial activity or kills bacteria, solving the shortcomings of active zinc oxide in artificial leather application .
Smart Images

Figure CN118895671A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of artificial leather, and in particular to an antibacterial and antiviral artificial leather and a preparation method thereof. Background Art
[0002] Conventional antibacterial and antiviral leather mostly uses silver ions, and the antibacterial property of silver ions is to damage bacterial cell membranes and cell walls, affecting bacterial growth and reproduction; the antiviral property of silver ions is to destroy the protein shell and genome of the virus, thereby inhibiting viral replication and infection. Silver ions are also harmful to the human body and may cause side effects such as allergic reactions, renal damage, blood system toxicity, nervous system toxicity, and skin burns.
[0003] Active zinc oxide is a new type of material that is being developed and used as a bactericidal material. It forms holes by receiving energetic photons, and then robs the hydroxyl electrons around the holes to turn them into free radicals, thereby completing the degradation of organic matter and killing bacteria and viruses.
[0004] However, the usage scenarios of active zinc oxide are demanding. When the energy carried by the photons is insufficient or the specific surface area is insufficient, the bactericidal effect will be affected. The environment in which artificial leather used in cars is located cannot avoid the above defects, so the application of active zinc oxide in artificial leather remains only in the theoretical stage.
[0005] Therefore, in order to further improve the bactericidal ability of artificial leather that is non-toxic to the human body, it is necessary to design an artificial leather containing active zinc oxide that can be used in a car environment. Summary of the invention
[0006] The invention provides an antibacterial and antiviral artificial leather and a preparation method thereof, so as to solve the problem that the existing bactericidal artificial leather containing active zinc oxide cannot be used in a car.
[0007] In order to solve the above technical problems, the present invention provides an antibacterial and antiviral artificial leather, comprising: a base fabric, an adhesive layer, a foaming layer and a surface layer stacked in sequence from top to bottom; wherein the surface layer comprises an antibacterial and antiviral agent containing active zinc oxide, a powder ammonia resistance agent and an ultraviolet light absorber; and the foaming layer comprises an antibacterial and antiviral agent.
[0008] Furthermore, the antibacterial concentration threshold of the active zinc oxide in the antibacterial and antiviral agent containing active zinc oxide is 200-400 ppm; the average particle size of the active zinc oxide single particle is 20 nm, the average diameter of the aggregate is 920 nm, and the specific surface area is ≥50 m 2 / g; and Pb<5ppm, Hg, As, Mn and Cd<1ppm in the antibacterial and antiviral agent.
[0009] Furthermore, the surface layer includes the following components in parts by mass: 43-48 parts of PVC powder; 38-43 parts of plasticizer; 1.8-2.2 parts of stabilizer; 3.6-4.2 parts of antibacterial and antiviral agent containing active zinc oxide; 0.3-0.7 parts of powder ammonia resistance agent; 5.5-6.0 parts of pigment; 0.2-0.4 parts of ultraviolet light absorber; and 3.0-3.5 parts of filler.
[0010] Furthermore, the foaming layer includes the following components in parts by weight: 43-48 parts of PVC powder; 35-40 parts of plasticizer; 1.1-1.5 parts of stabilizer; 1.7-2.1 parts of antibacterial and antiviral agent; 0.3-0.6 parts of pigment; 1.2-1.6 parts of flame retardant; and 9.0-11.0 parts of filler.
[0011] Furthermore, the adhesive layer comprises the following components in parts by weight: 53-58 parts of PVC powder; 40-45 parts of plasticizer; and 1-1.5 parts of stabilizer.
[0012] On the other hand, the present invention also provides a method for preparing an antibacterial and antiviral artificial leather, comprising the following steps: step S1: preparing coating materials for a surface layer, a foaming layer and an adhesive layer respectively in proportion; step S2, applying and drying the coating material prepared in step S1 on the surface of a release paper in sequence to obtain a base cloth, an adhesive layer, a foaming layer and a surface layer stacked in sequence from top to bottom; step S3, preparing a printing base coating and a printing surface coating in proportion; step S4, printing the printing base coating and the printing surface coating on the surface layer in sequence with a printing roller to obtain a semi-finished product; step S5, preheating the semi-finished product prepared in step S4, pressing out a pattern, and then cooling it to room temperature with a cooling roller and rolling it up to obtain the antibacterial and antiviral artificial leather as described above.
[0013] Further, the step S2 specifically includes the following steps: S21, evenly scraping the surface coating material prepared in step S1 on the surface of the release paper with a thickness of 35 filaments, baking at a temperature of 170-190°C for 48-60 seconds, and cooling to room temperature through a cooling roller after exiting the oven to obtain a surface layer; S22, evenly scraping the foaming layer coating material prepared in step S1 on the surface of the surface layer with a thickness of 40 filaments, baking at a temperature of 150-1 65℃, baking time is 48-60s, and after coming out of the oven, it is cooled to room temperature by cooling rollers to obtain a foaming layer; S23, the adhesive layer coating material prepared in step S1 is evenly scraped on the surface of the foaming layer with a thickness of 10 silks, and the base cloth is attached to the adhesive layer, and baked at a temperature of 190-210℃, and the baking time is 80-100s. After coming out of the oven, it is cooled to room temperature by cooling rollers to obtain a base cloth, an adhesive layer, a foaming layer and a surface layer stacked in sequence from top to bottom.
[0014] Furthermore, the step S3 specifically includes the following steps: S31, stirring and mixing in a proportion of 100 parts of a matte surface treatment agent, 3.5-4.5 parts of a curing agent, and 1.8-2.2 parts of an antibacterial and antiviral agent, and obtaining a printed base coating in an environment of 5-35°C; S32, stirring and mixing in a proportion of 65-75 parts of a matte surface treatment agent, 25-35 parts of a surface treatment agent, 3-4 parts of a curing agent, 1.8-2.2 parts of an antibacterial and antiviral agent, and 2-3 parts of an auxiliary agent, and obtaining a printed surface coating in an environment of 5-35°C.
[0015] Furthermore, the step S4 specifically includes the following steps: S41, using a 120-mesh printing roller to evenly print the printing base coating on the surface of the coated surface layer, baking at a temperature of 130-140°C for 35-50s, and cooling to room temperature via a cooling roller after exiting the oven to obtain a printing base layer; S42, using a 150-mesh printing roller to evenly print the printing base coating on the surface of the coated surface layer, baking at a temperature of 130-140°C for 40-55s, and cooling to room temperature via a cooling roller after exiting the oven to obtain a printing surface layer.
[0016] Furthermore, in step S5: the preheating temperature is 160-170° C., and the embossing speed is 15 m / min.
[0017] The beneficial effects of the present invention are that the antibacterial and antiviral artificial leather and the preparation method thereof of the present invention form an organic combination by arranging an antibacterial and antiviral agent containing active zinc oxide, a powder ammonia resistance agent and an ultraviolet light absorber in the surface layer, and converting ultraviolet light into visible light through the ultraviolet light absorber, which not only improves the yellowing problem of artificial leather, but also provides light energy for the active zinc oxide, so that it can receive as many photons as possible under the blocking of the automobile thermal insulation film; in addition, the powder ammonia resistance agent further improves the ammonia resistance effect while also increasing the specific surface area of the active zinc oxide, and the spherical zinc oxide has a large number of surface defects, which can activate the O in the environment. 2 and H 2 O, produces O 2 - and OH - Ions, O 2 - and OH - Ions attack the surface of bacteria or viruses, taking H and O from the bacterial membrane structure. 2 - and OH - The ions combine with the H element to form H 2 O and returns to the environment. Active zinc oxide destroys the membrane structure of bacteria through this pathway, thereby inhibiting bacterial activity or killing bacteria, thus realizing the application of bactericidal artificial leather containing active zinc oxide in automobiles.
[0018] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and the drawings.
[0019] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 The process flow chart of the preparation method of the antibacterial and antiviral artificial leather involved in some embodiments is shown. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] At least one embodiment provides an antibacterial and antiviral artificial leather, comprising: a base fabric, an adhesive layer, a foaming layer and a surface layer stacked in sequence from top to bottom; wherein the surface layer comprises an antibacterial and antiviral agent containing active zinc oxide, a powder ammonia resistance agent and an ultraviolet light absorber; and the foaming layer comprises an antibacterial and antiviral agent.
[0024] In this embodiment, specifically, the antibacterial concentration threshold of the active zinc oxide in the antibacterial and antiviral agent containing active zinc oxide is 200-400 ppm; the average particle size of the single active zinc oxide particle is 20 nm, the average diameter of the aggregate is 920 nm, and the specific surface area is ≥50 m 2 / g; and Pb<5ppm, Hg, As, Mn and Cd<1ppm in the antibacterial and antiviral agent.
[0025] In this embodiment, specifically, the surface layer includes the following components in parts by mass: 43-48 parts of PVC powder; 38-43 parts of plasticizer; 1.8-2.2 parts of stabilizer; 3.6-4.2 parts of antibacterial and antiviral agent containing active zinc oxide; 0.3-0.7 parts of powder ammonia resistance agent; 5.5-6.0 parts of pigment; 0.2-0.4 parts of ultraviolet light absorber; and 3.0-3.5 parts of filler.
[0026] In this embodiment, specifically, the foaming layer includes the following components in parts by weight: 43-48 parts of PVC powder; 35-40 parts of plasticizer; 1.1-1.5 parts of stabilizer; 1.7-2.1 parts of antibacterial and antiviral agent; 0.3-0.6 parts of pigment; 1.2-1.6 parts of flame retardant; and 9.0-11.0 parts of filler.
[0027] In this embodiment, specifically, the adhesive layer includes the following components in parts by weight: 53-58 parts of PVC powder; 40-45 parts of plasticizer; and 1-1.5 parts of stabilizer.
[0028] In this embodiment, specifically, the ammonia resistant agent is selected: the original traditional domestic barium zinc liquid ammonia resistant agent is an organic auxiliary agent with unstable properties; it is now replaced by a new powder ammonia resistant agent imported from abroad, which is an inorganic auxiliary agent, contains perchlorate, has stable properties, excellent ammonia resistance, and can increase the specific surface area of artificial leather.
[0029] In this embodiment, specifically, the selection of stabilizers: calcium zinc stabilizers are used in all three layers.
[0030] In this embodiment, specifically, the selection of plasticizer: a straight-chain plasticizer with a relatively large molecular weight (above 400) is selected.
[0031] In this embodiment, specifically, the selection of PVC powder is: selecting PVC paste resin with a higher degree of polymerization.
[0032] In this embodiment, specifically, inorganic pigments having stable molecular structures and excellent heat resistance are selected.
[0033] In this embodiment, specifically, the surface treatment agent is selected by selecting polyurethane with good heat resistance and light resistance.
[0034] In this embodiment, specifically, the antibacterial and antiviral agent: uses bio-based materials, is safe and environmentally friendly, is combined with active zinc oxide on the surface layer to enhance the bactericidal effect, and is set in the foaming layer to extend the bactericidal effect of artificial leather.
[0035] In this embodiment, specifically, the appropriate combination ratio is as follows: the raw materials are combined according to the above ratio to form a highly stable whole with long-lasting and superior antibacterial and antiviral properties.
[0036] like Figure 1As shown, at least one embodiment provides a method for preparing an antibacterial and antiviral artificial leather, comprising the following steps: step S1: preparing coating materials for a surface layer, a foaming layer and an adhesive layer respectively in proportion; step S2, applying and drying the coating material prepared in step S1 on the surface of a release paper in sequence to obtain a base cloth, an adhesive layer, a foaming layer and a surface layer stacked in sequence from top to bottom; step S3, preparing a printing base coating and a printing surface coating in proportion; step S4, printing the printing base coating and the printing surface coating on the surface layer in sequence with a printing roller to obtain a semi-finished product; step S5, preheating the semi-finished product prepared in step S4, pressing out a pattern, and then cooling it to room temperature with a cooling roller and rolling it up to obtain the antibacterial and antiviral artificial leather as described above.
[0037] Example 1
[0038] Step S1 (coating ingredients):
[0039] S11 surface layer: (by proportion) PVC powder B101145 parts, plasticizer C141040 parts, stabilizer D12102 parts, compound antibacterial and antiviral agent L2 containing active zinc oxide1104 parts, ammonia resistance agent D15100.5 parts, pigment G10105.8 parts, ultraviolet light absorber D12140.3 parts, filler D12143.3 parts.
[0040] First add PVC powder to the weighed plasticizer while stirring at a speed of 1100r / min. After stirring evenly, add it to the mixing barrel in descending order. After stirring evenly, vacuum degas the prepared slurry with a vacuum pressure of ≤-0.1Mpa for 30min and a stirring temperature of ≤45℃.
[0041] S12 foaming layer: (by proportion) PVC powder B101145 parts, plasticizer C141038 parts, stabilizer D12101.3 parts, antibacterial and antiviral agent L21101.9 parts, pigment G10100.5 parts, flame retardant H10101.4 parts, filler D121410 parts.
[0042] First add PVC powder to the weighed plasticizer, add while stirring, the stirring speed is 1100r / min, after stirring evenly, add it into the mixing bucket in order from most to least, stir evenly, and control the stirring temperature ≤45℃.
[0043] S13 bonding layer: (by proportion) PVC powder B101155 parts, plasticizer C141043 parts, stabilizer D12101.3 parts.
[0044] First add PVC powder to the weighed plasticizer, add while stirring, the stirring speed is 1100r / min, after stirring evenly, add stabilizer, stir evenly, and control the stirring temperature ≤45℃.
[0045] Step S2 (coating):
[0046] The S21 surface layer is evenly scraped on the surface of the release paper with a thickness of 35 filaments, put into the oven, the temperature is set to 170-190℃, the baking time is 48-60S, the most suitable time is 52-55S, and after leaving the oven, it is cooled to room temperature through a cooling roller;
[0047] The S22 foaming layer is evenly scraped on the surface of the surface layer with a thickness of 40 filaments, put into the oven, the temperature is set to 150-165°C, the baking time is 48-60S, the most suitable time is 52-55S, and after leaving the oven, it is cooled to room temperature through a cooling roller;
[0048] The S23 adhesive layer is evenly scraped on the surface of the foaming layer with a thickness of 10 threads, and the base cloth is flatly attached to the adhesive layer. It is put into the oven, the temperature is set to 190-210℃, the baking time is 80-100S, and the most suitable time is 90-95S. After leaving the oven, it is cooled to room temperature through a cooling roller, peeled off from the release paper and rolled up.
[0049] Step S3 (printing ingredients):
[0050] S31 printing bottom layer (by proportion): matte surface treatment agent J1012100 parts, curing agent K10104 parts, antibacterial and antiviral agent 2 parts;
[0051] After adding the curing agent into the weighed matte surface treatment agent, stir at a speed of 500r / min for 5-10min to mix evenly, and control the temperature between 5-35℃.
[0052] S32 printing surface layer (by proportion): 70 parts of matte surface treatment agent J1010, 30 parts of surface treatment agent J1011, 3.5 parts of curing agent K1010, 2 parts of antibacterial and antiviral agent L2110, and 2 to 3 parts of other additives.
[0053] First, mix the matte surface treatment agent and the surface treatment agent evenly at a stirring speed of 500r / min. After stirring evenly, add them into the mixing barrel in order from most to least, stir evenly, and control the temperature between 5-35℃.
[0054] Step S4 (printing):
[0055] S41 uses a 120-mesh printing roller to evenly print the printed bottom layer on the surface of the coated surface layer, puts it into an oven, sets the temperature to 130-140°C, bakes for 35-50 seconds, and the most suitable time is 42-45 seconds. After leaving the oven, it is cooled to room temperature through a cooling roller;
[0056] S42 uses a 150-mesh printing roller to print the printed surface layer by layer evenly on the surface of the printed bottom layer, puts it into an oven, sets the temperature to 130-140°C, and bakes it for 40-55 seconds, with the most suitable time being 45-50 seconds. After leaving the oven, it is cooled to room temperature by a cooling roller and rolled up;
[0057] Step S5 (embossing): the printed semi-finished product is put into an oven for preheating at a temperature of 160-170° C. and a speed of 15 m / min to emboss the pattern, and then cooled to room temperature by a cooling roller and rolled up to obtain the antibacterial and antiviral artificial leather.
[0058] Step S6 (inspection): inspect the synthetic leather according to the standard, trim and roll it up, and pack it for storage.
[0059] Example 2
[0060] Step S1 (coating ingredients):
[0061] S11 surface layer: (by proportion) PVC powder B101145 parts, plasticizer C141040 parts, stabilizer D12101.8 parts, compound antibacterial and antiviral agent L2110 containing active zinc oxide 3.8 parts, ammonia resistance agent D15100.3 parts, pigment G10105.8 parts, ultraviolet light absorber D12140.2 parts, filler D12143.3 parts.
[0062] First add PVC powder to the weighed plasticizer while stirring at a speed of 1100r / min. After stirring evenly, add it to the mixing barrel in descending order. After stirring evenly, vacuum degas the prepared slurry with a vacuum pressure of ≤-0.1Mpa for 30min and a stirring temperature of ≤45℃.
[0063] S12 foaming layer: (by proportion) PVC powder B101145 parts, plasticizer C141038 parts, stabilizer D12101.1 parts, antibacterial and antiviral agent L21101.7 parts, pigment G10100.5 parts, flame retardant H10101.4 parts, filler D121410 parts.
[0064] First add PVC powder to the weighed plasticizer, add while stirring, the stirring speed is 1100r / min, after stirring evenly, add it into the mixing bucket in order from most to least, stir evenly, and control the stirring temperature ≤45℃.
[0065] S13 bonding layer: (by proportion) PVC powder B101155 parts, plasticizer C141043 parts, stabilizer D12101.1 parts.
[0066] First add PVC powder to the weighed plasticizer, add while stirring, the stirring speed is 1100r / min, after stirring evenly, add stabilizer, stir evenly, and control the stirring temperature ≤45℃.
[0067] Step S2 (coating):
[0068] The S21 surface layer is evenly scraped on the surface of the release paper with a thickness of 35 filaments, put into the oven, the temperature is set to 170-190℃, the baking time is 48-60S, the most suitable time is 52-55S, and after leaving the oven, it is cooled to room temperature through a cooling roller;
[0069] The S22 foaming layer is evenly scraped on the surface of the surface layer with a thickness of 40 filaments, put into the oven, the temperature is set to 150-165°C, the baking time is 48-60S, the most suitable time is 52-55S, and after leaving the oven, it is cooled to room temperature through a cooling roller;
[0070] The S23 adhesive layer is evenly scraped on the surface of the foaming layer with a thickness of 10 threads, and the base cloth is flatly attached to the adhesive layer. It is put into the oven, the temperature is set to 190-210℃, the baking time is 80-100S, and the most suitable time is 90-95S. After leaving the oven, it is cooled to room temperature through a cooling roller, peeled off from the release paper and rolled up.
[0071] Step S3 (printing ingredients):
[0072] S31 printing bottom layer (by proportion): matte surface treatment agent J1012100 parts, curing agent K10104 parts, antibacterial and antiviral agent 1.8 parts;
[0073] After adding the curing agent into the weighed matte surface treatment agent, stir at a speed of 500r / min for 5-10min to mix evenly, and control the temperature between 5-35℃.
[0074] S32 printing surface layer (by proportion): 70 parts of matte surface treatment agent J1010, 30 parts of surface treatment agent J1011, 3.5 parts of curing agent K1010, 1.8 parts of antibacterial and antiviral agent L2110, and 2 to 3 parts of other additives.
[0075] First, mix the matte surface treatment agent and the surface treatment agent evenly at a stirring speed of 500r / min. After stirring evenly, add them into the mixing barrel in order from most to least, stir evenly, and control the temperature between 5-35℃.
[0076] Step S4 (printing):
[0077] S41 uses a 120-mesh printing roller to evenly print the printed bottom layer on the surface of the coated surface layer, puts it into an oven, sets the temperature to 130-140°C, bakes for 35-50 seconds, and the most suitable time is 42-45 seconds. After leaving the oven, it is cooled to room temperature through a cooling roller;
[0078] S42 uses a 150-mesh printing roller to print the printed surface layer by layer evenly on the surface of the printed bottom layer, puts it into an oven, sets the temperature to 130-140°C, and bakes it for 40-55 seconds, with the most suitable time being 45-50 seconds. After leaving the oven, it is cooled to room temperature by a cooling roller and rolled up;
[0079] Step S5 (embossing): the printed semi-finished product is put into an oven for preheating at a temperature of 160-170° C. and a speed of 15 m / min to emboss the pattern, and then cooled to room temperature by a cooling roller and rolled up to obtain the antibacterial and antiviral artificial leather.
[0080] Step S6 (inspection): inspect the synthetic leather according to the standard, trim and roll it up, and pack it for storage.
[0081] Example 3
[0082] Step S1 (coating ingredients):
[0083] S11 surface layer: (by proportion) PVC powder B101145 parts, plasticizer C141040 parts, stabilizer D12102.3 parts, compound antibacterial and antiviral agent L2110 containing active zinc oxide 4.2 parts, ammonia resistance agent D15100.7 parts, pigment G10105.8 parts, ultraviolet light absorber D12140.5 parts, filler D12143.3 parts.
[0084] First add PVC powder to the weighed plasticizer while stirring at a speed of 1100r / min. After stirring evenly, add it to the mixing barrel in descending order. After stirring evenly, vacuum degas the prepared slurry with a vacuum pressure of ≤-0.1Mpa for 30min and a stirring temperature of ≤45℃.
[0085] S12 foaming layer: (by proportion) PVC powder B101145 parts, plasticizer C141038 parts, stabilizer D12101.5 parts, antibacterial and antiviral agent L21102.1 parts, pigment G10100.5 parts, flame retardant H10101.6 parts, filler D121410 parts.
[0086] First add PVC powder to the weighed plasticizer, add while stirring, the stirring speed is 1100r / min, after stirring evenly, add it into the mixing bucket in order from most to least, stir evenly, and control the stirring temperature ≤45℃.
[0087] S13 bonding layer: (by proportion) PVC powder B101155 parts, plasticizer C141043 parts, stabilizer D12101.5 parts.
[0088] First add PVC powder to the weighed plasticizer, add while stirring, the stirring speed is 1100r / min, after stirring evenly, add stabilizer, stir evenly, and control the stirring temperature ≤45℃.
[0089] Step S2 (coating):
[0090] The S21 surface layer is evenly scraped on the surface of the release paper with a thickness of 35 filaments, put into the oven, the temperature is set to 170-190℃, the baking time is 48-60S, the most suitable time is 52-55S, and after leaving the oven, it is cooled to room temperature through a cooling roller;
[0091] The S22 foaming layer is evenly scraped on the surface of the surface layer with a thickness of 40 filaments, put into the oven, the temperature is set to 150-165°C, the baking time is 48-60S, the most suitable time is 52-55S, and after leaving the oven, it is cooled to room temperature through a cooling roller;
[0092] The S23 adhesive layer is evenly scraped on the surface of the foaming layer with a thickness of 10 threads, and the base cloth is flatly attached to the adhesive layer. It is put into the oven, the temperature is set to 190-210℃, the baking time is 80-100S, and the most suitable time is 90-95S. After leaving the oven, it is cooled to room temperature through a cooling roller, peeled off from the release paper and rolled up.
[0093] Step S3 (printing ingredients):
[0094] S31 printing bottom layer (by proportion): matte surface treatment agent J1012100 parts, curing agent K10104 parts, antibacterial and antiviral agent 2.2 parts;
[0095] After adding the curing agent into the weighed matte surface treatment agent, stir at a speed of 500r / min for 5-10min to mix evenly, and control the temperature between 5-35℃.
[0096] S32 printing surface layer (by proportion): 70 parts of matte surface treatment agent J1010, 30 parts of surface treatment agent J1011, 3.5 parts of curing agent K1010, 2.2 parts of antibacterial and antiviral agent L2110, and 2 to 3 parts of other additives.
[0097] First, mix the matte surface treatment agent and the surface treatment agent evenly at a stirring speed of 500r / min. After stirring evenly, add them into the mixing barrel in order from most to least, stir evenly, and control the temperature between 5-35℃.
[0098] Step S4 (printing):
[0099] S41 uses a 120-mesh printing roller to evenly print the printed bottom layer on the surface of the coated surface layer, puts it into an oven, sets the temperature to 130-140°C, bakes for 35-50 seconds, and the most suitable time is 42-45 seconds. After leaving the oven, it is cooled to room temperature through a cooling roller;
[0100] S42 uses a 150-mesh printing roller to print the printed surface layer by layer evenly on the surface of the printed bottom layer, puts it into an oven, sets the temperature to 130-140°C, and bakes it for 40-55 seconds, with the most suitable time being 45-50 seconds. After leaving the oven, it is cooled to room temperature by a cooling roller and rolled up;
[0101] Step S5 (embossing): the printed semi-finished product is put into an oven for preheating at a temperature of 160-170° C. and a speed of 15 m / min to emboss the pattern, and then cooled to room temperature by a cooling roller and rolled up to obtain the antibacterial and antiviral artificial leather.
[0102] Step S6 (inspection): inspect the synthetic leather according to the standard, trim and roll it up, and pack it for storage.
[0103] The antibacterial and antiviral artificial leathers obtained in Examples 1-3 and blank control samples were subjected to antibacterial and antiviral tests, and the results are shown in Tables 1 and 2 below, wherein Table 1 is a performance table of the antibacterial rates of Examples 1-3 and blank control samples, and Table 2 is a performance table of the antiviral activity rates of Example 1 and blank control samples.
[0104] Table 1
[0105]
[0106] Specifically, Escherichia coli is Escherichia coli AS1.90.
[0107] Specifically, Staphylococcus aureus is Staphylococcus aureus ATCC6538P.
[0108] Table 2
[0109]
[0110] Specifically, the Escherichia coli is Escherichia coli ATCC 8739.
[0111] Specifically, Staphylococcus aureus is Staphylococcus aureus ATCC6538P.
[0112] Table 3
[0113]
[0114]
[0115] The influenza A virus H1N1 is specifically influenza A virus H1N1: A / PR / 8 / 34 (ATCC VR-1469).
[0116] Specifically, the data in Table 1 are taken from the analysis and test results with report number 2021FM07952R01 issued by Guangdong Provincial Microbiological Analysis and Testing Center; the data in Table 2 are taken from the analysis and test results with report number ASH21-077673-01 issued by SGS Standards Technical Services (Shanghai) Co., Ltd.; the data in Table 3 are taken from the analysis and inspection results with report number 2021FM10865R01 issued by Guangdong Provincial Microbiological Analysis and Testing Center.
[0117] In summary, the antibacterial and antiviral artificial leather and the preparation method thereof of the present invention form an organic combination by arranging an antibacterial and antiviral agent containing active zinc oxide, a powder ammonia resistance agent and an ultraviolet light absorber in the surface layer, and converting ultraviolet rays into visible light through the ultraviolet light absorber, which not only improves the yellowing problem of artificial leather, but also provides light energy for the active zinc oxide, so that it can receive as many photons as possible under the blocking of the automobile thermal insulation film; in addition, the powder ammonia resistance agent further improves the ammonia resistance effect while also increasing the specific surface area of the active zinc oxide. The spherical zinc oxide has a large number of surface defects, which can activate the O in the environment. 2 and H 2 O, produces O 2 - and OH - Ions, O 2 - and OH - Ions attack the surface of bacteria or viruses, taking H and O from the bacterial membrane structure. 2 - and OH - The ions combine with the H element to form H 2 O and returns to the environment. Active zinc oxide destroys the membrane structure of bacteria through this pathway, thereby inhibiting bacterial activity or killing bacteria, thus realizing the application of bactericidal artificial leather containing active zinc oxide in automobiles.
[0118] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. An antibacterial and antiviral artificial leather, characterized in that: include: A base fabric, an adhesive layer, a foaming layer and a surface layer are stacked in sequence from top to bottom; in The surface layer includes an antibacterial and antiviral agent containing active zinc oxide, a powder ammonia resistance agent and an ultraviolet light absorber; The foaming layer includes an antibacterial and antiviral agent.
2. The antibacterial and antiviral artificial leather according to claim 1, characterized in that: The antibacterial concentration threshold of active zinc oxide in the antibacterial and antiviral agent containing active zinc oxide is 200-400 ppm; The average particle size of the active zinc oxide single particle is 20nm, the average diameter of the aggregate is 920nm, and the specific surface area is ≥50m 2 / g; as well as The antibacterial and antiviral agent contains Pb less than 5 ppm, and Hg, As, Mn and Cd less than 1 ppm.
3. The antibacterial and antiviral artificial leather according to claim 1, characterized in that: The surface layer comprises the following components in parts by weight: PVC powder 43-48 parts; 38-43 parts of plasticizer; Stabilizer 1.8-2.2 parts; 3.6-4.2 parts of antibacterial and antiviral agent containing active zinc oxide; Powder ammonia resistance agent 0.3-0.7 parts; Pigment 5.5-6.0 parts; 0.2-0.4 parts of ultraviolet light absorber; 3.0-3.5 parts of filler.
4. The antibacterial and antiviral artificial leather according to claim 1, characterized in that: The foaming layer comprises the following components in parts by weight: PVC powder 43-48 parts; 35-40 parts of plasticizer; Stabilizer 1.1-1.5 parts; 1.7-2.1 parts of antibacterial and antiviral agents; Pigment 0.3-0.6 parts; Flame retardant 1.2-1.6 parts; Filler 9.0-11.0 parts.
5. The antibacterial and antiviral artificial leather according to claim 1, characterized in that: The adhesive layer comprises the following components in parts by weight: PVC powder 53-58 parts; 40-45 parts of plasticizer; Stabilizer 1-1.5 parts.
6. A method for preparing antibacterial and antiviral artificial leather, characterized in that: The steps include: Step S1: preparing coating materials for the surface layer, the foaming layer and the adhesive layer respectively according to proportions; Step S2, applying the coating material prepared in step S1 on the surface of the release paper in sequence by scraping and drying to obtain a base fabric, an adhesive layer, a foaming layer and a surface layer stacked in sequence from top to bottom; Step S3, preparing the printing bottom layer coating and the printing surface layer coating according to the proportion; Step S4, printing the bottom coating and the surface coating on the surface layer in sequence with a printing roller to obtain a semi-finished product; Step S5, preheating the semi-finished product obtained in step S4, pressing out patterns, cooling it to room temperature through cooling rollers and rolling it up to obtain the antibacterial and antiviral artificial leather as claimed in claim 1.
7. The preparation method according to claim 6, characterized in that: The step S2 specifically includes the following steps: S21, evenly scrape the surface coating material prepared in step S1 on the surface of the release paper with a thickness of 35 filaments, bake at a temperature of 170-190° C. for 48-60 seconds, and cool to room temperature via a cooling roller after exiting the oven to obtain a surface layer; S22, evenly scrape the foaming layer coating material prepared in step S1 on the surface of the surface layer with a thickness of 40 threads, bake at a temperature of 150-165° C. for 48-60 seconds, and cool to room temperature via a cooling roller after exiting the oven to obtain a foaming layer; S23, evenly scrape the adhesive layer coating material prepared in step S1 on the surface of the foaming layer with a thickness of 10 silks, and stick the base fabric on the adhesive layer, bake at a temperature of 190-210 ° C, and bake for 80-100 seconds. After exiting the oven, cool to room temperature with a cooling roller to obtain a base fabric, adhesive layer, foaming layer and surface layer stacked in sequence from top to bottom.
8. The preparation method according to claim 6, characterized in that: The step S3 specifically includes the following steps: S31, mixing 100 parts of a matte surface treatment agent, 3.5-4.5 parts of a curing agent, and 1.8-2.2 parts of an antibacterial and antiviral agent in a ratio of 1.0 to 2.5, and obtaining a printing base coating at 5-35° C.; S32, stirring and mixing the matte surface treatment agent in a ratio of 65-75 parts, the surface treatment agent in a ratio of 25-35 parts, the curing agent in a ratio of 3-4 parts, the antibacterial and antiviral agent in a ratio of 1.8-2.2 parts, and the auxiliary agent in a ratio of 2-3 parts, and obtaining a printed surface coating at 5-35°C.
9. The preparation method according to claim 6, characterized in that: The step S4 specifically includes the following steps: S41, using a 120-mesh printing roller to evenly print the printing base coating on the surface of the coated surface layer, baking at a temperature of 130-140° C. for 35-50 seconds, and cooling to room temperature via a cooling roller after exiting the oven to obtain a printing base layer; S42, using a 150 mesh printing roller to evenly print the printing primer on the surface of the coated surface layer, baking at a temperature of 130-140° C. for 40-55 seconds, and cooling to room temperature via a cooling roller after exiting the oven to obtain a printed surface layer.
10. The preparation method according to claim 6, characterized in that: In step S5: The preheating temperature is 160-170°C and the embossing speed is 15m / min.