Production process of high-barrier plastic packaging paper for food

By forming barrier film and barrier layers in food packaging paper, the existing packaging paper is solved, and the existing packaging paper is insufficient protection in humid environments and high cost of degradable plastics is achieved, and the packaging paper with high barrier properties and air tightness is achieved to ensure food quality And reduce production costs.

CN118895679APending Publication Date: 2024-11-05FOSHAN XINFEI SANITARY MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411043302.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The barrier properties and protective properties of existing food packaging paper are insufficient, especially in humid environments, which are prone to erosion by water vapor, resulting in the inability to effectively protect the internal products. The production cost of biodegradable plastic materials is high, making it difficult to widely replace difficult-to-degradable plastics.

Method used

Using a production process of high-barrier plastic packaging paper for food, the barrier film and pulp fibers are formed by mixing components such as ethylene acrylic acid copolymer emulsion, sodium polyacrylate, tapioca oxidized starch and sodium carboxymethylcellulose. The base paper fiber increases waterproofness and flexibility, and sprays a second mixed emulsion on the paper to form a barrier layer to improve the barrier properties and airtightness of the wrapping paper.

Benefits of technology

It realizes good waterproofness, airtightness and mechanical strength of packaging paper, can effectively block food from the external environment, maintain food quality, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a production process of high-barrier plastic packaging paper for food, and belongs to the technical field of packaging papers.The production process comprises the following steps that S1, paper pulp raw materials are processed into papermaking fine pulp; s2, mixing an ethylene acrylic acid copolymer emulsion, sodium polyacrylate, cassava oxidized starch and sodium carboxymethyl cellulose to prepare a first mixed emulsion; s3, mixing the papermaking fine pulp with the first mixed emulsion to obtain papermaking primary pulp; s4, performing papermaking on the papermaking raw pulp, removing moisture, and drying to obtain coarse base paper; s5, mixing an ethylene acrylic acid copolymer emulsion, cassava oxidized starch, sodium carboxymethyl cellulose, purified water, sodium bicarbonate and a mixed additive to prepare a second mixed emulsion; s6, spraying the second mixed emulsion on the surface of the coarse base paper, drying, and calendering to obtain the packaging paper; the packaging paper disclosed by the invention has good barrier property, and when the packaging paper is used for packaging food, the food can be well isolated from the outside.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging paper, and in particular to a production process of high-barrier plastic-substitute packaging paper for food. Background Art

[0002] At present, the outer packaging of most food products is made of non-degradable plastic materials, which are prone to cause a series of microplastic hazards, namely plastic debris and particles with a diameter of less than 5mm, which can further turn into micron plastic, submicron plastic, and nanoplastic. Due to their tiny size and difficult to degrade properties, microplastics can easily enter the human body through the food chain, posing potential hazards to human health. Some of the outer packaging currently on the market is made of degradable plastics such as polylactic acid, polycaprolactone, and polypropylene succinate, but the production cost of these materials is high, making it difficult for them to widely replace difficult-to-degrade plastics and be used to make product outer packaging.

[0003] Wood pulp paper, as a product made of natural raw materials, is completely degradable, making it an ideal packaging material. However, the barrier and protective properties of current packaging paper and plastic packaging materials are quite different. Packaging paper is easily corroded by water vapor in a humid environment for a long time, and it is difficult for packaging paper to protect the products in the package from external factors such as water vapor for a long time. At present, some packaging papers are obtained by coating degradable barrier materials on the surface of wood pulp paper to form a waterproof barrier layer, thereby improving the long-term protective performance of the packaging paper. However, the non-waterproof nature of wood pulp paper itself has not changed. If the barrier layer is unevenly coated or the bonding strength between the barrier layer and the wood pulp paper is insufficient, the packaging paper may crack, delaminate, etc., which will make the internal wood pulp paper easily corroded by water vapor, resulting in the packaging paper being unable to protect the internal products well.

[0004] A Chinese patent with publication number CN111923546A discloses an environmentally friendly degradable waterproof coating packaging paper and a preparation method thereof, which is formed by co-extruding an inner layer, an intermediate layer and an outer layer onto a paper substrate in sequence, wherein the inner layer contains a polyvinyl alcohol acid copolymer and thermoplastic starch, the intermediate layer contains polyvinyl alcohol, thermoplastic starch, a plasticizer, a compatibilizer and other additives, and the outer layer contains a degradable polyester copolymer, thermoplastic starch, polydioxanone, a plasticizer, a compatibilizer and other additives; the packaging paper is made of natural renewable raw materials, so it has biodegradable properties, and It has the advantages of being waterproof and oil-proof, but the inner layer, middle layer and outer layer of the wrapping paper are all films made by a cast film process, and then the inner layer, middle layer and outer layer are compounded with a paper substrate in sequence to obtain the wrapping paper, but the paper substrate inside the wrapping paper itself does not have the properties of being waterproof and oil-proof. If delamination, cracking and the like occur during use, the paper substrate will be easily penetrated by external liquids such as moisture, and the liquid will also easily penetrate into the paper substrate through the edge of the wrapping paper, thereby reducing the strength of the wrapping paper or even causing damage. Therefore, there is still room for improvement in this wrapping paper. Summary of the invention

[0005] In view of the technical defects existing in the background technology, the present invention proposes a production process of high-barrier plastic-substitute packaging paper for food, which solves the above technical problems and meets the actual needs. The specific technical solution is as follows: A production process of high-barrier plastic-substitute packaging paper for food, comprising the following steps: S1, pulping, sand removal and grinding the pulp raw material to obtain papermaking rough pulp, and the papermaking rough pulp is subjected to primary pulping, sand removal and secondary pulping to obtain papermaking fine pulp; S2, mixing ethylene acrylic acid copolymer emulsion, sodium polyacrylate, oxidized tapioca starch and sodium carboxymethyl cellulose and stirring them uniformly and heating them for gelatinization to obtain a first mixed emulsion; S3, heating the papermaking fine pulp, adding the first mixed emulsion, mixing and stirring evenly to obtain papermaking stock pulp; S4, spreading the papermaking pulp on the surface of the screen through a headbox and shaping it through a finishing roller, waiting for the water of the papermaking pulp on the screen surface to drip naturally and cool down, then squeezing the papermaking pulp to remove excess water, preliminarily shaping it, and then drying it to obtain a coarse base paper; S5, mixing and stirring the ethylene acrylic acid copolymer emulsion, oxidized cassava starch, sodium carboxymethyl cellulose, purified water, sodium bicarbonate, and a mixing aid uniformly and heating and gelatinizing to obtain a second mixed emulsion; S6, spraying the second mixed emulsion evenly on the surface of the coarse base paper and allowing the second mixed emulsion to penetrate into the inside of the coarse base paper by oscillation, recovering the excess second mixed emulsion on the surface of the coarse base paper by a scraper and then drying it, and calendering the dried coarse base paper to obtain packaging paper.

[0006] As a further technical solution of the present invention, the pulp raw material includes the following components by mass percentage: 50%~70% coniferous wood pulp, 15%~30% broadleaf wood pulp, 10%~25% cotton pulp, 1%~2% polyamide-epichlorohydrin resin, and 0.1%~0.2% polyethylene oxide.

[0007] As a further technical solution of the present invention, in step S1, the papermaking raw pulp is subjected to pulp beating treatment in a post-beating pulp tank after the grinding operation, and the pulp beating degree ranges from 50 to 70oSR.

[0008] As a further technical solution of the present invention, the first mixed emulsion includes the following components by mass percentage: 50% to 70% ethylene acrylic acid copolymer emulsion, 20% to 30% sodium polyacrylate, 5% to 15% oxidized cassava starch, and 3% to 7% sodium carboxymethyl cellulose.

[0009] As a further technical solution of the present invention, the solid content of the ethylene acrylic acid copolymer emulsion is 45% to 50%.

[0010] As a further technical solution of the present invention, in step S3, the temperature of heating the papermaking fine pulp is 50-80°C.

[0011] As a further technical solution of the present invention, in step S3, the first mixed emulsion and the papermaking fine pulp are mixed in a ratio of 1:50 to 1:5.

[0012] As a further technical solution of the present invention, the second mixed emulsion includes the following components by mass percentage: 30% to 50% ethylene acrylic acid copolymer emulsion, 5% to 10% oxidized cassava starch, 2% to 6% sodium carboxymethyl cellulose, 30% to 50% purified water, 1% to 5% sodium bicarbonate, and 0.5% to 2% mixing aid.

[0013] As a further technical solution of the present invention, the mixing auxiliary agent includes the following components in percentage by mass: 30% to 70% of dispersant and 30% to 70% of leveling agent.

[0014] As a further technical solution of the present invention, in step S6, the second mixed emulsion is sprayed on both the upper and lower surfaces of the coarse base paper, and the spraying amount of the second mixed emulsion on one side of the coarse base paper is 1-4 g / m 2 .

[0015] The beneficial effects of the present invention are: The present invention obtains coarse base paper by subjecting papermaking pulp to operations such as papermaking. The first mixed emulsion in the papermaking pulp forms a barrier film on the surface of pulp fibers. The barrier film and the pulp fibers together constitute base paper fibers. The barrier film enables the base paper fibers to have good waterproofness and flexibility. The sodium polyacrylate in the barrier film can block the gaps between the base paper fibers by swelling after absorbing water to prevent further penetration of water, so that the coarse base paper has good barrier performance and mechanical strength. Then, the second mixed emulsion is sprayed on the surface of the coarse base paper to form a barrier layer and obtain packaging paper, so that the packaging paper has good barrier properties, air tightness and surface smoothness. When the packaging paper is used to package food, the food can be well blocked from the outside world, so that the food maintains good quality. DETAILED DESCRIPTION

[0016] The implementation mode of the present invention is described below in conjunction with relevant embodiments. The implementation mode of the present invention is not limited to the following embodiments, and the present invention relates to relevant necessary components in the technical field, which should be regarded as the known technology in the technical field and can be known and mastered by the technical personnel in the technical field.

[0017] A production process of high-barrier plastic-substitute packaging paper for food, comprising the following steps: S1, pulping, sand removal and grinding the pulp raw material to obtain papermaking rough pulp, and the papermaking rough pulp is subjected to primary pulping, sand removal and secondary pulping to obtain papermaking fine pulp; S2, mixing ethylene acrylic acid copolymer emulsion, sodium polyacrylate, oxidized tapioca starch and sodium carboxymethyl cellulose and stirring them uniformly and heating them for gelatinization to obtain a first mixed emulsion; S3, heating the papermaking fine pulp, adding the first mixed emulsion, mixing and stirring evenly to obtain papermaking stock pulp; S4, spreading the papermaking pulp on the surface of the screen through a headbox and shaping it through a finishing roller, waiting for the water of the papermaking pulp on the screen surface to drip naturally and cool down, then squeezing the papermaking pulp to remove excess water, preliminarily shaping it, and then drying it to obtain a coarse base paper; S5, mixing and stirring the ethylene acrylic acid copolymer emulsion, oxidized cassava starch, sodium carboxymethyl cellulose, purified water, sodium bicarbonate, and a mixing aid uniformly and heating and gelatinizing to obtain a second mixed emulsion; S6, spraying the second mixed emulsion evenly on the surface of the coarse base paper and allowing the second mixed emulsion to penetrate into the inside of the coarse base paper by oscillation, recovering the excess second mixed emulsion on the surface of the coarse base paper by a scraper and then drying it, and calendering the dried coarse base paper to obtain packaging paper.

[0018] As one of the preferred embodiments of the present invention, the pulp raw material includes the following components by mass percentage: 50% to 70% of coniferous wood pulp, 15% to 30% of broadleaf wood pulp, 10% to 25% of cotton pulp, 1% to 2% of polyamide-epichlorohydrin resin, and 0.1% to 0.2% of polyethylene oxide; the above materials can be used as raw materials for manufacturing wood pulp paper, and these raw materials retain the effective components of papermaking and purify the papermaking quality during pulping and punching, and finally obtain wood pulp paper with good flexibility, stability and performance bonding; among them, coniferous wood pulp, broadleaf wood pulp and cotton pulp are common raw materials in the papermaking process and are the main components of pulp, providing a large amount of cellulose, lignin and other components for pulp, so that pulp can be processed through a series of processes The wood pulp paper is prepared after the steps; the polyamide-epichlorohydrin resin is mainly used as a wet strength agent in the pulp, and the polyamide-epichlorohydrin resin reacts with hydroxyl groups, aldehyde groups and the like on the surface of the pulp fiber through functional groups such as amino groups and epoxy groups to form a cross-linked structure and enhance the bonding force between the pulp fibers, thereby improving the wet strength of the wood pulp paper finally obtained, so that the wood pulp paper can still maintain good physical properties in a humid environment; the polyethylene oxide is mainly used as a dispersant in the pulp, and in the papermaking process, pulp fibers and other components are insoluble in water, and they tend to aggregate in water by themselves, and the addition of the dispersant can form a double-layer structure on the surface of the solid particles, and the outer layer dispersant has a strong affinity with water, thereby increasing the degree to which the solid particles are wetted by water and improving the dispersion effect of the pulp fibers.

[0019] In a further preferred embodiment based on the aforementioned embodiment, in step S1, the papermaking rough pulp is subjected to a beating treatment in a post-beating pulp pool after the grinding operation, and the pulp beating degree ranges from 50 to 70oSR; the papermaking rough pulp of the present invention is refined with a higher beating degree, and its pulp fibers are more effectively dispersed during the refining process, and the entanglement and aggregation between the pulp fibers are reduced, so that the pulp fibers are more evenly distributed in the papermaking rough pulp, which is beneficial to the interweaving and bonding of the pulp fibers in the subsequent papermaking process, and improves the uniformity and strength of wood pulp paper; in addition, during the refining process, the cell walls of the pulp fibers absorb water and swell, and at the same time, part of the cell walls are broken, exposing more hydrophilic groups such as hydroxyl groups, making it easier for the pulp fibers to combine with water molecules, and the pulp with a high beating degree usually has a higher swelling and hydration degree of the pulp fibers, which is beneficial to the bonding between the pulp fibers and the forming of the paper.

[0020] The papermaking coarse pulp of the present invention is subjected to primary pulping, sand removal, and secondary pulping to obtain papermaking fine pulp, which can be made into common wood pulp paper through subsequent processes such as papermaking. However, the strength, water resistance and other properties of wood pulp paper are not excellent, making it difficult to be used as an ideal material for packaging paper. Therefore, the papermaking fine pulp needs to be further processed and a first mixed emulsion is added. The first mixed emulsion includes the following components by mass percentage: 50% to 70% of ethylene acrylic acid copolymer emulsion, 20% to 30% of sodium polyacrylate, 5% to 15% of cassava oxidized starch, and 3% to 7% of sodium carboxymethyl cellulose; an appropriate amount of water can be added to the first mixed emulsion, stirred evenly, and then heated to promote uniform dispersion, dissolution and gelatinization of each component.

[0021] It should be noted that after the first mixed emulsion is mixed with the papermaking fine pulp, it will disperse and dissolve in water to form papermaking raw pulp, and will gradually adsorb and penetrate into the pulp fibers during the stirring process. In the subsequent processing steps, the water content of the papermaking raw pulp is reduced so that the pulp fibers therein form the structure of wood pulp paper. In this process, the first mixed emulsion that penetrates into the pulp fibers will form a barrier film composed of ethylene acrylic acid copolymer, sodium polyacrylate, cassava oxidized starch, and sodium carboxymethyl cellulose and wrap the pulp fibers therein. The pulp fibers and the barrier film together constitute the base paper fibers, and a number of base paper fibers constitute the coarse base paper of the paper structure.

[0022] In the first mixed emulsion of the present invention, the ethylene acrylic acid copolymer emulsion is a high molecular polymer prepared by copolymerization of ethylene and acrylic acid monomers and dispersed in water to form a liquid, the solid content of the ethylene acrylic acid copolymer emulsion is 45% to 50%, the ethylene acrylic acid copolymer emulsion can be dissolved in water or can be dispersed in water, preferably soluble in water, the ethylene acrylic acid copolymer has good adhesion, water resistance and flexibility, so that the barrier film can be firmly bonded to the pulp fiber, and the barrier film can well prevent water penetration, improve the water resistance and flexibility of the base paper fiber, make the coarse base paper have good water resistance and flexibility, and avoid the strength reduction or even damage caused by water penetration; the base paper fibers in the coarse base paper are inevitably The base paper has tiny gaps to allow water to pass through. The sodium polyacrylate in the barrier film is in a dry state and has good water absorption. When water passes through the gaps between the base paper fibers, it will be absorbed by the sodium polyacrylate to prevent the coarse base paper from being penetrated by water. After absorbing water, the sodium polyacrylate will swell and block the gaps between the base paper fibers, so that the gaps between the base paper fibers have no capillary effect, thereby preventing water from continuing to penetrate and improving the waterproofness of the coarse base paper. Cassava oxidized starch, sodium carboxymethyl cellulose and ethylene acrylic acid copolymer all have good compatibility, which can improve the mechanical strength, film-forming properties, adhesion, biodegradability and other properties of the barrier film, so that the base paper fibers have good mechanical strength and achieve biodegradability, thereby improving environmental protection.

[0023] As one of the preferred embodiments of the present invention, in step S3, the temperature of heating the paper pulp is 50-80°C; after heating, the paper pulp can increase its solubility in the first mixed emulsion. After the first mixed emulsion is added to the paper pulp, the components in the first mixed emulsion can be evenly dispersed and dissolved in water to form paper pulp, and heating can reduce the viscosity of the paper pulp, so that the ethylene acrylic acid copolymer, sodium polyacrylate, oxidized cassava starch, and sodium carboxymethyl cellulose can better penetrate into the pulp fibers, which is beneficial to the subsequent formation of a barrier film on the surface of the pulp fibers.

[0024] In a further preferred embodiment based on the above embodiment, in step S4, the papermaking pulp is spread on the surface of the mesh curtain through the headbox and shaped by the finishing roller. The dry weight of the papermaking pulp after finishing needs to be maintained at 20g / m 2 As mentioned above, if the dry weight is too low, the coarse base paper produced is too thin and unsuitable as packaging paper. The actual dry weight is adaptively adjusted according to demand. The moisture of the paper pulp on the surface of the mesh curtain drips naturally and cools down to room temperature. During the cooling process, the viscosity of the paper pulp will increase. At the same time, the solubility of ethylene acrylic acid copolymer, sodium polyacrylate, cassava oxidized starch, and sodium carboxymethyl cellulose in water will decrease. Under the combined effect of these two factors, a gelatinous layer composed of ethylene acrylic acid copolymer, sodium polyacrylate, cassava oxidized starch, and sodium carboxymethyl cellulose gradually adheres to the surface of the pulp fiber. Then the paper pulp is pressed to remove excess moisture. During the pressing process, the gelatinous layer is still attached to the surface of the pulp fiber and is initially shaped into a base paper blank. Finally, the base paper blank is dried to dehydrate the gelatinous layer to form a barrier film. The barrier film and pulp fiber together constitute the coarse base paper.

[0025] As one of the preferred embodiments of the present invention, in step S3, the first mixed emulsion and the papermaking fine pulp are mixed in a ratio of 1:100 to 1:10; the papermaking fine pulp contains about 90% water, which facilitates the papermaking fine pulp to dissolve the first mixed emulsion to form papermaking stock pulp, and the proportion of ethylene acrylic acid copolymer, sodium polyacrylate, cassava oxidized starch, and sodium carboxymethyl cellulose in the papermaking stock pulp is preferably 2% to 5%, and the actual proportion needs to be adaptively adjusted according to the required performance of the coarse base paper. A high proportion of these components in the papermaking stock pulp can form a thicker barrier film on the surface of the pulp fiber, reduce the gaps between the base paper fibers in the coarse base paper and improve the barrier properties of the coarse base paper, but the heating temperature of the papermaking stock pulp needs to be increased, and the viscosity of the papermaking stock pulp will be increased, requiring a greater pressing pressure, thereby increasing the energy consumption and process difficulty in the papermaking process, and increasing the manufacturing cost of the coarse base paper.

[0026] In a further preferred embodiment based on the aforementioned embodiment, in step S4, the water removed from the papermaking stock is used as white water for adjusting the concentration of papermaking fine pulp; before pulping in step S1, the papermaking coarse pulp is mixed with the white water and subjected to one pulping, sand removal, and a second pulping to obtain the papermaking fine pulp. Since the white water still contains a certain amount of ethylene acrylic acid copolymer, sodium polyacrylate, oxidized cassava starch, and sodium carboxymethyl cellulose, these components can be recovered by adjusting the concentration with white water, thereby reducing the papermaking cost. In the following step S3, it is necessary to reduce the amount of the first mixed emulsion added. The purpose of adding the first mixed emulsion is to supplement the common content of ethylene acrylic acid copolymer, sodium polyacrylate, oxidized cassava starch, and sodium carboxymethyl cellulose in the papermaking stock to within a set range, thereby ensuring the performance of the coarse base paper.

[0027] As one of the preferred embodiments of the present invention, the second mixed emulsion includes the following components in mass percentage: 30%~50% ethylene acrylic acid copolymer emulsion, 5%~10% cassava oxidized starch, 2%~6% sodium carboxymethyl cellulose, 30%~50% purified water, 1%~5% sodium bicarbonate, and 0.5%~2% mixing aid; the second mixed emulsion is used to penetrate into the gaps between the base paper fibers in the coarse base paper, forming a barrier layer on the surface of the coarse base paper, avoiding structures such as capillaries on the surface of the coarse base paper, so that the surface of the final packaging paper is smoother and has better barrier properties.

[0028] In the second mixed emulsion of the present invention, the ethylene acrylic acid copolymer emulsion is a high molecular polymer prepared by copolymerization of ethylene and acrylic acid monomers and dispersed in water to form a liquid, the solid content of the ethylene acrylic acid copolymer emulsion is 45% to 50%, the ethylene acrylic acid copolymer emulsion can be dissolved in water or can be dispersed in water, preferably soluble in water, the ethylene acrylic acid copolymer has good adhesion, water resistance, and flexibility, and can make the barrier layer firmly adhere to the surface of the coarse base paper to form packaging paper, improve the waterproofness and flexibility of the packaging paper, and avoid the packaging paper from being reduced in strength or even damaged due to water penetration; the cassava oxidized starch, sodium carboxymethyl cellulose and the ethylene acrylic acid copolymer all have good compatibility, which can improve the mechanical properties of the barrier layer. The second mixed emulsion improves the mechanical strength, film-forming property, adhesion, biodegradability and other properties, so that the base paper fibers have good mechanical strength and biodegradability, and improve environmental protection; pure water is used as a solvent and diluent in the second mixed emulsion, and the cassava oxidized starch, sodium carboxymethyl cellulose, sodium bicarbonate and other components are dissolved by the pure water, and the viscosity of the second mixed emulsion is reduced by the dilution effect of the pure water, so that the second mixed emulsion is easier to coat and penetrate into the gaps between the base paper fibers; sodium bicarbonate is used to adjust the pH of the second mixed emulsion to make the second mixed emulsion alkaline, so that the second mixed emulsion maintains a high solubility for the ethylene acrylic acid copolymer, avoids the precipitation of the ethylene acrylic acid copolymer, and improves the stability of the mixed system in the second mixed emulsion.

[0029] In a further preferred embodiment based on the aforementioned embodiment, the mixing aid includes the following components in mass percentage: 30% to 70% dispersant and 30% to 70% leveling agent; the dispersant may be selected from dispersants with surface activity such as fatty acid salts, sulfonates, and phosphates, and the dispersant may help to evenly disperse some insoluble solid particles in the liquid to prevent particle aggregation and precipitation; the leveling agent is preferably an organosilicon leveling agent, and the organosilicon leveling agent may improve the wettability and leveling effect of the second mixed emulsion, and good wettability enables the second mixed emulsion to better contact with the coarse base paper and reduce defects caused by poor wetting, and good leveling effect helps the second mixed emulsion to form a uniform and smooth barrier layer on the surface of the coarse base paper, avoids defects such as shrinkage holes and orange peel in the barrier layer, and improves the flatness of the packaging paper surface.

[0030] As one of the preferred embodiments of the present invention, in step S6, the second mixed emulsion needs to be sprayed on both the upper and lower surfaces of the coarse base paper, and the spraying amount of the second mixed emulsion on one side of the coarse base paper is 1-4 g / m 2 The solid content of the second mixed emulsion is in the range of 30% to 50%. The viscosity of the second mixed emulsion can be reduced by reducing the solid content of the second mixed emulsion or increasing the temperature to make it easier to coat on the surface of the coarse base paper. The barrier layer formed after the second mixed emulsion is cured serves as a structure to strengthen the barrier properties of the packaging paper surface, ensuring that the solid content of the second mixed emulsion sprayed on one side of the coarse base paper is 0.5 to 1 g / m 2 range; in addition, after the second mixed emulsion is sprayed on the surface of the coarse base paper, the ultrasonic vibration equipment can be used to generate vibration to promote the second mixed emulsion to penetrate into the gaps between the base paper fibers, so that the first mixed emulsion can form a barrier layer to improve the bonding strength with the coarse base paper, and improve the air tightness and barrier properties of the packaging paper.

[0031] In summary, the present invention obtains coarse base paper by subjecting papermaking pulp to operations such as papermaking, the first mixed emulsion in the papermaking pulp forms a barrier film on the surface of pulp fibers, the barrier film and pulp fibers together constitute base paper fibers, the barrier film enables the base paper fibers to have good waterproofness and flexibility, the sodium polyacrylate in the barrier film can block the gaps between the base paper fibers by swelling after absorbing water to prevent further penetration of water, so that the coarse base paper has good barrier properties and mechanical strength, then the second mixed emulsion is sprayed on the surface of the coarse base paper to form a barrier layer and obtain packaging paper, so that the packaging paper has good barrier properties, air tightness, and surface smoothness. When the packaging paper is used to package food, the food can be well blocked from the outside world, so that the food maintains good quality.

[0032] The present invention is further described below by way of examples and comparative examples.

[0033] Example 1

[0034] S1, pulping, sand removal and grinding the pulp raw materials to obtain papermaking rough pulp, and the papermaking rough pulp is subjected to primary pulping, sand removal and secondary pulping to obtain papermaking fine pulp; the pulp raw materials include the following components by mass percentage: 60% of coniferous wood pulp, 20% of hardwood pulp, 18.3% of cotton pulp, 1.5% of polyamide-epichlorohydrin resin, and 0.2% of polyethylene oxide; the moisture content of the papermaking fine pulp is 90%; S2, mixing 60% of ethylene acrylic acid copolymer emulsion, 25% of sodium polyacrylate, 10% of oxidized tapioca starch, and 5% of sodium carboxymethyl cellulose by mass, stirring evenly, and heating and gelatinizing to obtain a first mixed emulsion; S3, heating the papermaking fine pulp and mixing it with the first mixed emulsion at a mass ratio of 10:1 to obtain papermaking stock; S4, spreading the papermaking pulp on the surface of the screen through a headbox and shaping it through a finishing roller, waiting for the water of the papermaking pulp on the screen surface to drip naturally and cool down, then squeezing the papermaking pulp to remove excess water, preliminarily shaping it, and then drying it to obtain a coarse base paper; S5, mixing 40% of ethylene acrylic acid copolymer emulsion, 7% of oxidized tapioca starch, 4% of sodium carboxymethyl cellulose, 45% of purified water, 3% of sodium bicarbonate, 0.5% of dispersant, and 0.5% of leveling agent by mass, stirring and heating to gelatinize to obtain a second mixed emulsion; S6, the second mixed emulsion was prepared at 2.5 g / m 2 The coating amount is evenly sprayed on the surface of the coarse base paper and the second mixed emulsion is allowed to penetrate into the interior of the coarse base paper by oscillation. The excess second mixed emulsion on the surface of the coarse base paper is recovered by a scraper and then dried. The dried coarse base paper is calendered to obtain packaging paper.

[0035] Example 2

[0036] The difference between this embodiment and the above-mentioned embodiment 1 is that in step S3, the papermaking fine pulp is heated and then mixed with the first mixed emulsion at a mass ratio of 20:1 and stirred to obtain papermaking raw pulp, and the operations of the remaining steps are the same.

[0037] Example 3

[0038] The difference between this embodiment and the above-mentioned embodiment 1 is that in step S3, the papermaking fine pulp is heated and then mixed with the first mixed emulsion at a mass ratio of 30:1 and stirred evenly to obtain papermaking raw pulp, and the operations of the remaining steps are the same.

[0039] Example 4

[0040] The difference between this embodiment and the above-mentioned embodiment 1 is that in step S3, the papermaking fine pulp is heated and then mixed with the first mixed emulsion at a mass ratio of 40:1 and stirred to obtain papermaking raw pulp, and the operations of the remaining steps are the same.

[0041] It should be noted that in order to make the content of the first mixed emulsion in the papermaking pulp more accurate, no white water is added to the papermaking pulp in all the above embodiments. Only when white water is added to the papermaking pulp will a lower proportion of the first mixed emulsion be added. Therefore, the papermaking pulp with a lower content of the first mixed emulsion is not listed in the above embodiments.

[0042] Comparative Example 1 The packaging paper was obtained with reference to Example 4 in the specification of Chinese patent "An environmentally friendly degradable waterproof coating packaging paper and its preparation method" (publication number: CN111923546A).

[0043] It should be noted that the weight of the packaging paper obtained in all the above examples and comparative examples is 50 g / m 2 .

[0044] The wrapping papers obtained in all the above embodiments and comparative examples were tested for mechanical properties and waterproof properties. The mechanical properties of the wrapping papers were specifically tested for tensile strength and elongation at break, and the waterproof properties of the wrapping papers were specifically tested for water vapor permeability. The test results are shown in Table 1 below:

[0045] Table 1 The packaging papers obtained in all the above embodiments and comparative examples were fixed in the working area of ​​the vibration tester. After the vibration tester was started until the packaging paper was delaminated, the waterproof performance of the packaging paper was tested. The waterproof performance of the packaging paper was specifically tested for water vapor permeability. The test results are shown in Table 2 below:

[0046] Table 2 According to the analysis of the data in Table 1, in Examples 1-4 based on the technical solution of the present invention, as the content of the first mixed emulsion in the papermaking pulp increases, the mechanical properties and waterproof properties of the wrapping paper are better, because the increase in the content of the first mixed emulsion will form a thicker barrier film on the surface of the pulp fiber, so that the wrapping paper has higher tensile strength and elongation at break, and the thicker barrier film can make the base paper fibers more tightly bonded, and the effect of water absorption by sodium polyacrylate is better, so the waterproof property of the wrapping paper is better; while in Comparative Example 1, the mechanical properties and waterproof properties of the wrapping paper mainly depend on the three-layer film. In the process of testing the mechanical properties, when the paper substrate is completely torn and the wrapping paper can no longer be used as a packaging material, the wrapping paper is regarded as torn. Although the paper substrate can ensure that the wrapping paper has certain mechanical properties, the defect of poor flexibility makes it easy to be torn. Once the paper substrate is torn, it will make it difficult for the wrapping paper to provide good protection for the packaged products.

[0047] According to the analysis of the data in Table 2, after the packaging paper is vibrated until it is delaminated by the vibration testing machine, the situation of the packaging paper after friction and collision during use can be simulated. In Examples 1-4, the water vapor permeability of the packaging paper increases by 2-4 times after vibration, while the water vapor permeability of the packaging paper of Comparative Example 1 increases by more than 5 times after vibration. It can be seen that the packaging paper obtained based on the technical solution of the present invention can still play a good protective role for the packaged products during use.

[0048] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A production process for high barrier plastic packaging paper for food, characterized in that: The following steps are involved: S1, pulping, sand removal and grinding the pulp raw material to obtain papermaking rough pulp, and the papermaking rough pulp is subjected to primary pulping, sand removal and secondary pulping to obtain papermaking fine pulp; S2, mixing ethylene acrylic acid copolymer emulsion, sodium polyacrylate, oxidized tapioca starch and sodium carboxymethyl cellulose and stirring them uniformly and heating them for gelatinization to obtain a first mixed emulsion; S3, heating the papermaking fine pulp, adding the first mixed emulsion, mixing and stirring evenly to obtain papermaking raw pulp; S4, spreading the papermaking pulp on the surface of the screen through a headbox and shaping it through a finishing roller, waiting for the water of the papermaking pulp on the screen surface to drip naturally and cool down, then squeezing the papermaking pulp to remove excess water, preliminarily shaping it, and then drying it to obtain a coarse base paper; S5, mixing and stirring the ethylene acrylic acid copolymer emulsion, oxidized cassava starch, sodium carboxymethyl cellulose, purified water, sodium bicarbonate, and a mixing aid uniformly and heating and gelatinizing to obtain a second mixed emulsion; S6, spraying the second mixed emulsion evenly on the surface of the coarse base paper and allowing the second mixed emulsion to penetrate into the inside of the coarse base paper by oscillation, recovering the excess second mixed emulsion on the surface of the coarse base paper by a scraper and then drying it, and calendering the dried coarse base paper to obtain packaging paper.

2. The production process of high barrier plastic-substitute packaging paper for food according to claim 1, characterized in that: The pulp raw material includes the following components by mass percentage: 50% to 70% of softwood pulp, 15% to 30% of hardwood pulp, 10% to 25% of cotton pulp, 1% to 2% of polyamide-epichlorohydrin resin, and 0.1% to 0.2% of polyethylene oxide.

3. The production process of high barrier plastic packaging paper for food according to claim 1, characterized in that: In step S1, the papermaking raw pulp is subjected to pulp beating treatment in a post-beating pulp tank after the grinding operation, and the pulp beating degree ranges from 50 to 70°SR.

4. The production process of high barrier plastic-substitute packaging paper for food according to claim 1, characterized in that: The first mixed emulsion includes the following components by mass percentage: 50% to 70% ethylene acrylic acid copolymer emulsion, 20% to 30% sodium polyacrylate, 5% to 15% oxidized cassava starch, and 3% to 7% sodium carboxymethyl cellulose.

5. The production process of high barrier plastic packaging paper for food according to claim 1, characterized in that: The solid content of the ethylene acrylic acid copolymer emulsion is 45% to 50%.

6. The production process of high barrier plastic substitute packaging paper for food according to claim 1, characterized in that: In step S3, the temperature of heating the papermaking fine pulp is 50-80°C.

7. The production process of high barrier plastic-substitute packaging paper for food according to claim 1, characterized in that: In step S3, the first mixed emulsion and the papermaking fine pulp are mixed in a ratio of 1:50 to 1:

5.

8. The production process of high barrier plastic-substitute packaging paper for food according to claim 1, characterized in that: The second mixed emulsion includes the following components by mass percentage: 30% to 50% ethylene acrylic acid copolymer emulsion, 5% to 10% cassava oxidized starch, 2% to 6% sodium carboxymethyl cellulose, 30% to 50% purified water, 1% to 5% sodium bicarbonate, and 0.5% to 2% mixing aid.

9. The production process of high barrier plastic-substitute packaging paper for food according to claim 1, characterized in that: The mixing auxiliary agent includes the following components by mass percentage: 30% to 70% of a dispersant and 30% to 70% of a leveling agent.

10. The production process of high barrier plastic-substitute packaging paper for food according to claim 1, characterized in that: In step S6, the second mixed emulsion is sprayed on both the upper and lower surfaces of the coarse base paper, and the spraying amount of the second mixed emulsion on one side of the coarse base paper is 1-4 g / m 2 .