Overlying strata separation layer grouting method and slurry runout disposal method

By using slurry containing tracer, fly ash and cement slurry in the rock-covered rock-covered destrata grouting project, the problem of slurry running accidents during rock-covered destrata grouting is solved, and the problem of slurry running accidents is achieved. Safe and efficient production recovery.

CN118895953APending Publication Date: 2024-11-05CHINA COAL SCI & ENG ECOLOGICAL ENVIRONMENT TECH CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411157965.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the rock-covered off-stratum grouting project, under the long-term high pressure, the first slurry may conduct along the cracks or faults, resulting in slurry accidents and affecting the progress and safety of the operation.

Method used

A rock-covered destratum grouting method is adopted to observe the water inflow of underground and ground, and inject slurry containing tracer into the drill hole for sealing, calculate the amount of sealing slurry, and combine the use of fly ash and cement slurry. Gradually seal the cracks and set up casing assemblies in the drilling structure and location design to prevent slurry run.

Benefits of technology

The cracks are sealed in a timely and effective manner, ensuring that the drilling holes are not blocked, reducing accident losses and casualties, and ensuring production recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895953A_ABST
    Figure CN118895953A_ABST
Patent Text Reader

Abstract

The invention discloses an overlying strata separation layer grouting method which comprises a slurry runout disposal method, the slurry runout disposal method comprises an underground slurry runout disposal method, and the underground slurry runout disposal method comprises the steps that the underground water inflow and the slurry runout amount are observed; when the grout running amount is larger than the water inflow amount, grout containing a tracer agent is injected into the drill hole, the grout is injected into the drill hole in multiple times for plugging, the interval of grouting every time is preset time, and the calculation formula of the volume of the grout injected into the drill hole is V seal = alpha (Q1 + Q2 +... Qn). T / 1000, and V seal represents the plugging grout use amount / m < 3 >; q1, Q2,... Qn respectively represent the grouting flow / (L / min) of each drill hole when grout runout occurs, and n is greater than or equal to 1; t is the time / min from starting to press the tracer agent to detecting the tracer agent on the working surface after slurry leakage; alpha is a correction coefficient, and the value range of alpha is 0.3-0.9. According to the overlying strata separation layer grouting method provided by the embodiment of the invention, the crack can be effectively blocked in time, and the drilling hole is ensured not to be blocked.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of overburden rock separation layer grouting, and in particular to an overburden rock separation layer grouting method and a grout leakage treatment method. Background Art

[0002] The overburden delamination grouting project is a dynamic and comprehensive coordination process of underground working face coal mining and ground grouting. This process involves all systems related to the underground working face and the ground grouting system, and the grouting work is often accompanied by coal mining at the working face and even until the completion of the entire stage of sealing wall construction.

[0003] Overburden stratum grouting is a long-term pressurized grouting project. Under the action of long-term pressure, the first slurry diffuses to the pores between the stratum and the weak cracks in the stratum. Due to the impact of coal mining subsidence, on the one hand, some cracks in the stratum will develop to the surface. On the other hand, although there is a certain thickness of protective layer at the bottom of the borehole and the working surface, under the action of long-term high pressure, the first slurry may continue to seep and diffuse along the cracks. When it reaches a certain level, the cracks can be conducted. These two situations will cause the first slurry to run underground or to the ground, which is easy to cause production and safety accidents.

[0004] In addition, under the influence of special geological structures, the probability of grouting leakage in overburden separation grouting projects is greatly increased. For example, if there is a fault fracture zone near the working face, and the fault develops to the area above the roof, or even to the surface. Under the dual effects of high pressure of separation grouting and mining affecting the movement of overburden, the first grouting slurry may be conducted to the working face along the fault, or it may flow to the surface along the fault fracture zone, causing various grouting accidents, affecting the progress of the operation, and easily causing safety accidents. Therefore, the prevention and treatment of grouting leakage is particularly important. Summary of the invention

[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, an embodiment of the present invention provides a method for grouting a separation layer of an overburden rock, which can timely and effectively seal the cracks and ensure that the borehole is not blocked.

[0006] The overburden separation grouting method of the embodiment of the present invention includes: a slurry leakage treatment method, wherein the slurry leakage treatment method includes a treatment method for underground slurry leakage, and the treatment method for underground slurry leakage includes:

[0007] Observe the water inflow and slurry loss in the well;

[0008] When the slurry flow is greater than the water inflow, the slurry containing the tracer is injected into the borehole. The slurry is injected into the borehole several times for plugging. The interval between each grouting is preset. The volume of the slurry injected into the borehole is calculated as follows:

[0009] V 封 =α·(Q1+Q2+……Qn )·t / 1000

[0010] Where V 封 Indicates the amount of plugging slurry / m 3 ; Q1, Q2, ... Q n They represent the grouting flow rate of each borehole when slurry leakage occurs / (L / min), n≥1; t is the time from the beginning of injection of tracer to the detection of tracer on the working face after slurry leakage / min; α is the correction coefficient, and the value range of α is: 0.3~0.9.

[0011] The overburden separation grouting method of the embodiment of the present invention can timely and effectively seal the cracks for the treatment of slurry leakage in the well, ensure that the borehole is not blocked, and resume production in a short time, effectively reducing accident losses and casualties.

[0012] In some embodiments, the method for treating downhole slurry leakage further includes:

[0013] When the water inflow is greater than the slurry flow, inject fly ash slurry with a concentration greater than 75% into the borehole, observe the slurry inflow in the well, and if the slurry inflow in the well decreases or becomes clearer, continue to inject fly ash slurry with a concentration greater than 75% into the borehole;

[0014] If the slurry gushing out from the well does not decrease and does not become clear, inject cement slurry into the borehole, and the volume of cement slurry injected into the borehole is greater than the volume of the borehole, and then stop injecting fly ash slurry with a concentration greater than 75% into the borehole, then clean the borehole, observe the slurry gushing situation in the well at intervals of a preset time, if the amount of water gushing and slurry leakage in the well are reduced to the preset amount, inject fly ash slurry with a concentration greater than 75% into the borehole, otherwise perform multiple intermittent grouting into the borehole until there is no more slurry leakage in the well.

[0015] In some embodiments, the slurry leakage treatment method further includes a treatment method for slurry bubbling on the ground, and the treatment method for slurry bubbling on the ground includes:

[0016] S1, injecting clean water containing a tracer into the borehole, and stopping the water injection after confirming that the borehole is not blocked;

[0017] S2. Observe the tracer. When the tracer is observed in the borehole, calculate the volume V of the clean water containing the tracer injected. 清 , after a preset time interval, cement slurry or cement fly ash slurry is injected into the borehole multiple times, and the volume of the injected cement slurry or cement fly ash slurry is V 浆 , V 浆 >V 清, when the tracer cannot be observed in the borehole, cement slurry or cement fly ash slurry is injected into the borehole for plugging in multiple times and at a preset interval each time, and fly ash slurry with a concentration greater than 70% is injected into the borehole after plugging is completed. If slurry still occurs, the concentration of the cement slurry or cement fly ash slurry and the time interval of each time are increased. If slurry does not occur, fly ash slurry with a concentration greater than 70% is injected;

[0018] During the above process, the slurry bubbling situation at the slurry bubbling point is observed at all times. When the slurry at the slurry bubbling point flows back, cement slurry is injected into the slurry bubbling point until no more injection is possible.

[0019] In some embodiments, when the slurry flow rate is greater than the water inflow rate, the working surface after the borehole is first plugged is observed.

[0020] When no slurry or tracer is observed on the working surface, α is set between 0.5 and 0.9, and grouting is performed into the borehole in multiple times until plugging is completed;

[0021] When slurry or tracer is observed on the working surface, the borehole with slurry leakage is judged based on the pressure at the hole mouth, pump pressure value or pressure curve when the slurry is leaking. If it cannot be judged, α is taken between 0.3 and 0.5.

[0022] In some embodiments, when the grouting volume is greater than the water gushing volume, clean water containing a tracer is injected into the borehole. When no tracer is observed in the borehole, grouting into the borehole is stopped. After a preset time interval, cement slurry and plugging materials are injected into the borehole to seal the borehole.

[0023] In some embodiments, the overburden separation grouting method further includes a slurry leakage prevention method, and the slurry leakage prevention method includes:

[0024] When designing the drilling structure, the thickness H of the loose layer and the length L of the open hole section of the drilling hole are judged. When H is greater than a preset value and L is also greater than the preset value, the drilling hole passes through the loose layer and the bedrock layer in sequence, and the open hole section of the drilling hole is located below the bedrock layer. A casing assembly is arranged in the drilling hole, and the casing assembly includes a first cement casing, a surface casing, a second cement casing and a technical casing. The first cement casing is arranged in the loose layer, the surface casing is arranged inside the first cement casing and around the inner circumference of the first cement casing, the second cement casing is arranged inside the surface casing and around the inner circumference of the surface casing, the technical casing is arranged inside the second cement casing and extends to the bedrock layer, and the technical casing is arranged around the inner circumference of the second cement casing;

[0025] When designing the drilling position, it is determined that the drilling is directional drilling, and the drilling offset position is arranged perpendicular to the working face mining direction or the drilling position is arranged in the opposite direction to the working face mining direction.

[0026] In some embodiments, the method for preventing pulp runaway further comprises:

[0027] When a fault exists, analyzing the section affected by the fault on the borehole, and if the section affected by the fault on the borehole is in the bedrock layer or below the bedrock layer, extending the borehole to below the bedrock layer, and setting a casing assembly in the borehole to isolate the section affected by the fault outside the technical casing;

[0028] When a fault is present, the borehole is extended above the affected section of the fault.

[0029] In some embodiments, the method for preventing pulp runaway further comprises:

[0030] When the casing assembly is arranged in the borehole, a reserved section is arranged at the lower end of the technical casing, and the reserved section can be extended and retracted relative to the technical casing along the extension direction of the technical casing. When the lower end of the technical casing receives ground stress, the reserved section is extended to extend the technical casing;

[0031] After the drilling is completed, if the analysis shows that the drilling does not meet the grouting conditions, a water pressure test is carried out in the drilling, and if the orifice pressure is lower than the preset orifice pressure, the drilling is sealed.

[0032] The slurry leakage treatment method according to an embodiment of the present invention comprises:

[0033] A method for treating slurry leakage in a well, wherein the method for treating slurry leakage in a well is the method for treating slurry leakage in a well as claimed in any one of claim 2, wherein when the water inflow is greater than the slurry leakage, the volume of cement slurry injected into the borehole is 2 to 4 times the volume of the borehole, and the preset interval time is greater than 8 hours;

[0034] A method for treating slurry on the ground, wherein the method for treating slurry on the ground is the method for treating slurry on the ground according to claim 3, wherein the preset interval time is greater than 12 hours, V 浆 =1.5~2V 清 .

[0035] The slurry leakage treatment method of the embodiment of the present invention can promptly and maturely handle the slurry leakage occurring under different working conditions, effectively seal the cracks, ensure that the borehole is not blocked, and reduce accident losses and casualties.

[0036] In some embodiments, when the slurry flow rate is greater than the water inflow rate, the volume of clean water containing the tracer injected into the borehole is 4 to 6 times the volume of the borehole. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a schematic diagram of a casing assembly of a grouting method for overburden separation according to an embodiment of the present invention.

[0038] Figure 2 It is a schematic diagram of the drilling structure and position adjustment under special geological structures of the overburden separation grouting method according to an embodiment of the present invention.

[0039] Figure 3 It is a schematic diagram of the drilling structure and position adjustment under special geological structures of the overburden separation grouting method according to an embodiment of the present invention.

[0040] Figure 4 It is a schematic diagram showing that the offset position of the drilling hole in the overburden separation grouting method according to an embodiment of the present invention is arranged perpendicular to the pushing and mining direction of the working face.

[0041] Figure 5 It is a schematic diagram showing that the offset position of the drilling hole in the overburden separation grouting method according to an embodiment of the present invention is arranged in a direction opposite to the pushing and mining direction of the working face.

[0042] Figure numerals: 100, borehole; 1, casing assembly; 11, first cement casing; 12, surface casing; 13, second cement casing; 14, technical casing; 15, reserved section; 21, loose layer; 22, bedrock layer. DETAILED DESCRIPTION

[0043] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0044] like Figure 1-5 As shown, the overburden separation grouting method of the embodiment of the present invention includes a slurry leakage treatment method, and the slurry leakage treatment method includes a treatment method for underground slurry leakage and a treatment method for surface slurry leakage.

[0045] Specifically, the treatment method for underground slurry leakage is:

[0046] ① If only the water inflow increases, or there is a small amount of slurry, and the slurry flow rate is less than 5m 3 / h, inject high-concentration fly ash slurry with a concentration greater than 75% into the borehole 100, and reasonably reduce the grouting flow rate, observe the slurry gushing situation underground, if the slurry running out is reduced or the slurry gradually becomes clear, continue to inject the high-concentration fly ash slurry.

[0047] If the grouting volume does not decrease and the grout does not become clear, the grouting should be stopped intermittently. Before stopping the grouting, 2 to 4 times of pure cement slurry with a specific gravity of 1.4 to 1.8 g / cm3 should be injected into the borehole at 100 volume. 3. After the pure cement slurry is injected, clean the borehole 100, and take an interval of more than 8 hours to observe the slurry inflow in the well. If the water and slurry output in the well decrease to normal, gradually resume normal grouting. In the initial stage of recovery, use a high-concentration fly ash slurry with a concentration greater than 75%, or add 5-25% cement, and use a high-concentration fly ash slurry in the transition. Otherwise, perform multiple intermittent injections of high-concentration fly ash slurry with a concentration greater than 75% until the slurry stops flowing.

[0048] ② If the amount of underground slurry is greater than the amount of water inflow, first determine the type of plugging slurry. According to the grouting field of the overburden separation layer and the need for water plugging / slurry, cement slurry, cement fly ash slurry and ultrafine cement slurry are used. Due to the large amount of underground slurry, cement slurry is preferred, followed by ultrafine cement slurry. The plugging amount of cement slurry is the key to this method. The plugging amount must be within a reasonable range or an accurate value. If the single plugging amount is insufficient, the cement slurry will be diluted by water and fly ash slurry in the formation, prolonging the plugging time and the time for subsequent restoration of grouting and underground coal mining. If the plugging amount is too large, the injected slurry will fill the slurry channel, and will spread along the cracks between the separation layer holes and around the borehole 100, and part of the cement slurry will enter the underground. In this case, the original normal grouting filling range will be blocked, affecting the grouting effect of the overburden separation layer of the borehole 100. At the same time, the cement slurry will bring many harmful factors to the underground.

[0049] The calculation method of cement slurry plugging dosage is:

[0050] V 封 =α·(Q1+Q2+……Q n )·t / 1000

[0051] Where V 封 Indicates the amount of plugging slurry / m 3 ; Q1, Q2, ... Q n They represent the grouting flow rate of each borehole 100 when slurry leakage occurs / (L / min), n≥1; t is the time from the beginning of the injection of tracers to the detection of tracers at the working face after slurry leakage / min; α is the correction coefficient, which is 0.3~0.9. Because of the injection of clean water containing tracers, after the grouting is stopped, the working face may be pushed and mined, and the fly ash slurry injected in the early stage will settle when there is no subsequent driving force, and the channels and cracks of slurry leakage are partially closed. After the grouting is stopped, the greater the recovery of the coal mining working face, the longer the time from the injection of clean water containing tracers to the stop of grouting, the smaller the value of α, so it needs to be determined comprehensively in combination with the formation, mine, and the actual situation of slurry leakage.

[0052] In some embodiments, when cement slurry is first injected for plugging, α is initially set to 0.5, and α·Q is injected into each borehole 100. n· t cubic meters of cement slurry, add tracer into the cement slurry, the tracer cannot react with cement slurry, add plugging material of 1% to 5% of cement mass each time the cement slurry is injected, the plugging material can be sawdust, slag lignin, walnut shell powder, high molecular polymer, etc., rest for more than 4 hours, and then carry out the second plugging.

[0053] After the first plugging is completed, observe whether cement slurry can be observed on the working face. If no cement slurry or tracer is observed, the value range of α is basically determined, and a larger value between 0.5 and 0.9 can be taken. Plug and observe successively until the plugging is completed.

[0054] If cement slurry or tracer is observed at the working face, analysis should be performed based on the orifice pressure, pump pressure value or pressure curve of each borehole 100 when slurry is leaking to determine the borehole 100 most likely to have slurry leaking. If the specific borehole 100 with slurry leaking cannot be determined, the value of α should be less than 0.5.

[0055] If it can be clearly determined that the drilling hole has slurry leakage 100, the plugging amount of cement slurry at this time can be expressed by the following formula:

[0056] V 封 =Q n t / 1000

[0057] This formula is equivalent to pressing pure cement slurry into a single borehole 100 to block the slurry leakage channel.

[0058] The premise of the above two formulas is that after the slurry leakage is discovered on the working face, the emergency plan is immediately activated, and the grouting pump in the slurry is placed in the clean water pool with tracer added to pressurize clean water containing tracer into each borehole 100. When the injection amount does not reach more than 2 times the volume of the borehole 100, the flow rate cannot be reduced, that is, the flow rate when the clean water is pressed in remains the same as the flow rate when the slurry leakage is discovered.

[0059] According to the above ①②, after plugging for 3 to 5 times, if there is no more slurry in the well, consider injecting low-flow, high-concentration fly ash slurry to gradually resume production. If there is still slurry in the well, the injection volume of cement slurry should be increased, and a small amount of accelerator should be considered. The amount of accelerator to be added should be subject to special tests.

[0060] ③If the method of step ② is adopted, 4 to 6 times the volume of clean water containing tracers has been injected into the borehole 100, and no tracers are found in the well, comprehensive disposal measures need to be taken. First, stop grouting for an interval to ensure that the underground working face resumes production as soon as possible, and gradually promote production by a uniform and continuous advancement method. Second, after an interval of 24h to 72h, use a plugging method of pure cement slurry plus plugging materials, and the volume of slurry injected each time is 2 to 5 times the volume of the borehole 100.

[0061] Specifically, the plugging material is added in an amount of 2% to 6% of the mass of cement, and the plugging material may be sawdust, slag lignin, walnut shell powder, high molecular polymer, and the like.

[0062] Specifically, the specific gravity of cement slurry is 1.4-1.8 g / cm 3 , carry out 3 to 5 pluggings, with an interval of more than 4 hours between each plugging, and observe the amount of slurry leakage from the working face. If the slurry leakage has not been significantly reduced, the injection amount of cement slurry should be increased, and consideration should be given to adding a small amount of accelerator. The amount of accelerator added should be subject to special tests.

[0063] If the slurry leakage is significantly reduced but can still be observed, considering that grouting needs to be resumed in the later stage of drilling 100, the method of injecting fly ash cement slurry is adopted. The initial cement ratio is relatively large, which should be greater than 30%. According to the amount of slurry leakage, it is reduced step by step, and the total amount of slurry injected each time can be gradually increased until there is no more slurry leakage. If there is no more slurry leakage on the working face after 3 to 5 pluggings, intermittent injection of bottom flow and high-concentration fly ash slurry is adopted, with an interval of 3 to 6 hours, and the amount of fly ash injected each time is gradually increased until production is fully restored.

[0064] In addition to the above steps ② and ③, there is a situation where the amount of slurry leakage is extremely large, which affects the safety of the mine. In this case, the above method cannot be adopted. It is necessary to adopt 100 cycles of grouting in the drilling to quickly release the formation pressure. When the conditions are met, the sealing method of step ③ can be adopted.

[0065] Specifically, the treatment method for ground slurry is:

[0066] ① First, observe and judge the characteristics of the slurry bubbling site. If the slurry bubbling site is a well, a borehole 100 or has point-like characteristics, the treatment method is:

[0067] In case of single hole grouting, clean water containing tracer is pressed into the borehole 100, and water injection is stopped after confirming that the borehole 100 is not blocked. If the tracer cannot be observed when the pump is stopped, cement slurry or cement fly ash slurry is injected from the borehole 100 in 2 to 4 times after an interval of more than 12 hours, with an interval of more than 4 hours each time. After the plugging is completed, fly ash slurry with a concentration greater than 70% is used for trial grouting. If there is still slurry bubbling, the concentration of cement slurry and the interval time of each time should be increased. If there is no continuous slurry bubbling, grouting is gradually resumed.

[0068] If the tracer can be observed when the pump is stopped, the volume of clean water containing the tracer V is calculated from the time when the tracer is observed as the node. 清 After a rest of more than 12 hours, cement slurry or cement fly ash slurry is injected from the borehole 100 in 2 to 4 times, each time with an interval of more than 4 hours, and the amount of slurry injected is V 清 1.5 to 2 times of.

[0069] If multiple holes are grouting at the same time, clean water containing tracers will be pressed into different batches to stop grouting. The time interval between each drilling 100 stops should be more than 30 minutes. After each drilling 100 stops, observe the slurry discharge from the slurry point and whether the tracer can be observed.

[0070] For the above-mentioned single-hole or multi-hole simultaneous grouting, cement slurry must be prepared in advance. When the slurry at the slurry point flows back, cement slurry is immediately poured in from that point until it cannot be poured in any further.

[0071] ② If the slurry bubbling part is in the form of flakes, strips or other irregular shapes, the treatment measures are the same as ①, but there is no need to prepare cement slurry for reinjection from the slurry bubbling point.

[0072] The overburden separation grouting method of the embodiment of the present invention also includes a slurry leakage prevention method. The slurry leakage prevention method is implemented from the following five technical perspectives.

[0073] 1. When designing the structure of the borehole 100, the thickness H of the loose layer 21 and the length L of the open hole section of the borehole 100 are judged. When H is greater than a preset value and L is also greater than a preset value, the borehole 100 passes through the loose layer 21 and the bedrock layer 22 in sequence, and the open hole section of the borehole 100 is located below the bedrock layer 22. A casing assembly 1 is arranged in the borehole 100, and the casing assembly 1 includes a first cement casing 11, a surface casing 12, a second cement casing 13 and a technical casing 14. The first cement casing 11 is arranged in the loose layer 21, the surface casing 12 is arranged inside the first cement casing 11 and around the inner circumference of the first cement casing 11, the second cement casing 13 is sleeved inside the surface casing 12 and around the inner circumference of the surface casing 12, the technical casing 14 is arranged in the second cement casing 13 and extends to the bedrock layer 22, and the technical casing 14 is arranged around the inner circumference of the second cement casing 13.

[0074] Specifically, the preset value is 40m. The loose layer 21 is miscellaneous fill, humus, gravel layer, etc. The bedrock layer 22 is located below the loose layer 21. The technical casing 14 isolates the loose layer 21 from the bedrock layer 22 under the multiple effects of the first cement casing 11, the surface casing 12, and the second cement casing 13, effectively preventing a certain layer of casing from being torn under the action of ground stress and preventing slurry from running to the ground.

[0075] 2. When designing the position of the borehole 100, it is determined that the borehole 100 is a directional borehole 100, and the offset position of the borehole 100 is arranged perpendicular to the mining direction of the working face or the borehole 100 is arranged in the direction opposite to the mining direction of the working face.

[0076] Specifically, the present invention gives priority to arranging the offset position of the borehole 100 perpendicular to the mining direction of the working face. If the above-mentioned hole arrangement conditions are not met due to the project progress, drilling construction period, etc., the position of the borehole 100 is designed to be opposite to the mining direction of the working face. These two arrangements weaken the ground stress effect caused by mining, thereby reducing damage to the borehole 100, reducing the probability of breaking the technical casing 14, and reducing the possibility of slurry leakage.

[0077] 3. When there is a fault, the section affected by the fault on the borehole 100 is analyzed. If the section affected by the fault on the borehole 100 is in the bedrock layer 22 or below the bedrock layer 22, the borehole 100 is extended to below the bedrock layer 22, and a casing assembly 1 is set in the borehole 100 to isolate the section affected by the fault outside the technical casing 14. Alternatively, the borehole 100 is extended above the section affected by the fault.

[0078] Specifically, if there are special geological structures such as faults and collapse columns, in order to prevent slurry from escaping from the faults or their surroundings, the design should be carried out from the following two points:

[0079] ① Analyze the impact section of the fault or other structure on the borehole 100. If the fault impact section is in the bedrock layer 22 or below the bedrock layer 22, the borehole 100 is still extended to below the bedrock layer 22 without affecting the grouting, and the fault is isolated outside the technical casing 14, thereby ensuring that the high-pressure slurry of the delamination grouting does not produce pressure shock on the fault, thereby preventing slurry leakage accidents underground and on the ground.

[0080] ② The landing point of borehole 100 is arranged above special geological structures such as faults and collapse columns without affecting the grouting effect. Borehole 100 does not pass through the fault zone to reduce the disturbance of high-pressure slurry to the fault zone. The slurry is located above the fault zone to reduce the probability of slurry leakage underground and on the ground.

[0081] Fourth, when the casing assembly 1 is set in the borehole 100, a reserved section 15 is set at the lower end of the technical casing 14. The reserved section 15 can be extended and retracted along the extension direction of the technical casing 14 relative to the technical casing 14. When the lower end of the technical casing 14 receives ground stress, the reserved section 15 is extended to extend the technical casing 14, thereby ensuring that the technical casing 14 is not broken and reducing the probability of slurry leakage.

[0082] 5. After the drilling hole 100 is completed, if it is analyzed that the drilling hole 100 does not meet the grouting conditions, a water pressure test is carried out in the drilling hole 100. If the orifice pressure is lower than the preset orifice pressure, the drilling hole 100 is blocked.

[0083] Specifically, if the analysis does not meet the separation grouting conditions, but the injection volume Q of the drilling 100 circulation fluid is large, greater than 10m 3 / h. Further measures are taken, namely, water pressure test. If the orifice pressure P is 0 or the water pressure V is 3 to 5 times greater than the volume of the borehole 100, and the flow rate Q is not less than 15m 3 / h, and the orifice pressure is still lower than the normal pore pressure, plugging measures are taken to prevent slurry leakage after grouting. The plugging measures are to use fly ash slurry with a concentration of 60-75%, add a certain amount of cement for plugging, and the amount of cement added is 5%-30% of the fly ash mass. The amount of slurry for each plugging is 1.5-3 times the volume of the borehole 100, and then pressurize the water intermittently. After plugging 2-3 times, if the water pressure test pressure P is still small or 0, pure cement slurry is used for intermittent grouting, and the amount of cement slurry injected each time is 1.5-3 times the volume of the borehole 100.

[0084] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0085] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0086] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0087] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0088] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0089] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A method for grouting overburden separation layer, characterized in that: include: A slurry leakage treatment method, wherein the slurry leakage treatment method includes a treatment method for underground slurry leakage, and the treatment method for underground slurry leakage includes: Observe the water inflow and slurry loss in the well; When the slurry flow rate is greater than the water inflow rate, a slurry containing a tracer is injected into the borehole (100). The slurry is injected into the borehole (100) for plugging multiple times. Each grouting interval is a preset time. The volume of the slurry injected into the borehole (100) is calculated as follows: V 封 =α·(Q1+Q2+……Q n )·t / 1000 Where V 封 Indicates the amount of plugging slurry / m 3 ; Q1, Q2, ... Q n They represent the grouting flow rate of each borehole (100) when slurry leakage occurs / (L / min), n≥1; t is the time from the beginning of injection of the tracer to the detection of the tracer on the working face after slurry leakage / min; α is the correction coefficient, and the value range of α is: 0.3~0.

9.

2. The overburden separation grouting method according to claim 1, characterized in that: The treatment methods for underground slurry leakage also include: When the amount of water gushing out is greater than the amount of slurry running out, injecting fly ash slurry with a concentration greater than 75% into the borehole (100), observing the slurry gushing out underground, and if the slurry gushing out underground decreases or the slurry gushing out gradually becomes clear, continue to inject fly ash slurry with a concentration greater than 75% into the borehole (100); If the slurry gushing out from the well does not decrease and does not become clear, cement slurry is injected into the borehole (100), and the volume of cement slurry injected into the borehole (100) is greater than the volume of the borehole (100), then the injection of fly ash slurry with a concentration greater than 75% into the borehole (100) is stopped, and then the borehole (100) is cleaned, and the slurry gushing situation in the well is observed at intervals of a preset time. If the amount of water gushing and the amount of slurry running out from the well are reduced to a preset amount, fly ash slurry with a concentration greater than 75% is injected into the borehole (100). Otherwise, multiple intermittent grouting operations are performed into the borehole (100) until there is no more slurry running out from the well.

3. The overburden separation grouting method according to claim 1, characterized in that: The slurry leakage treatment method also includes a treatment method for slurry bubbling on the ground, and the treatment method for slurry bubbling on the ground includes: S1, injecting clean water containing a tracer into the borehole (100), and stopping the water injection after confirming that the borehole (100) is not blocked; S2. Observe the tracer. When the tracer is observed in the borehole (100), calculate the volume V of the clean water containing the tracer injected. After a preset time interval, inject cement slurry or cement fly ash slurry into the borehole (100) multiple times. The volume of the cement slurry or cement fly ash slurry injected is V. 浆 , V 浆 >V 清 , when the tracer cannot be observed in the borehole (100), cement slurry or cement fly ash slurry is injected into the borehole (100) for plugging multiple times and at a preset time interval each time, and after the plugging is completed, fly ash slurry with a concentration greater than 70% is injected into the borehole (100). If slurry still occurs, the concentration of the cement slurry or cement fly ash slurry and the time interval of each time are increased. If slurry does not occur, fly ash slurry with a concentration greater than 70% is injected; During the above process, the slurry bubbling situation at the slurry bubbling point is observed at all times. When the slurry at the slurry bubbling point flows back, cement slurry is injected into the slurry bubbling point until no more injection is possible.

4. The overburden separation grouting method according to claim 1, characterized in that: When the slurry flow rate is greater than the water inflow rate, the working surface after the first plugging of the borehole (100) is observed. When no slurry or tracer is observed on the working surface, α is set between 0.5 and 0.9, and grouting is performed into the borehole (100) in multiple times until plugging is completed; When slurry or tracer is observed on the working surface, the borehole (100) where slurry is leaking is judged based on the pressure at the borehole mouth, pump pressure value or pressure curve when slurry is leaking. If it cannot be judged, α is taken between 0.3 and 0.

5.

5. The overburden separation grouting method according to claim 1, characterized in that: When the amount of grouting is greater than the amount of water gushing, clean water containing a tracer is injected into the borehole (100); when no tracer is observed in the borehole (100), grouting into the borehole (100) is stopped; after a preset time interval, cement slurry and plugging material are injected into the borehole (100) to seal the borehole (100).

6. The overburden separation grouting method according to claim 1, characterized in that: Also included is a pulp running prevention method, the pulp running prevention method comprising: When designing the structure of a borehole (100), the thickness H of the loose layer (21) and the length L of the open hole section of the borehole (100) are determined. When H is greater than a preset value and L is also greater than the preset value, the borehole (100) passes through the loose layer (21) and the bedrock layer (22) in sequence. The open hole section of the borehole (100) is located below the bedrock layer (22). A casing assembly (1) is arranged in the borehole (100). The casing assembly (1) comprises a first cement casing (11), a surface casing (12), a second cement casing (13) and a technical casing ( 14), the first cement casing (11) is arranged in the loose layer (21), the surface casing (12) is arranged inside the first cement casing (11) and around the inner circumference of the first cement casing (11), the second cement casing (13) is sleeved inside the surface casing (12) and around the inner circumference of the surface casing (12), the technical casing (14) is arranged in the second cement casing (13) and extends to the bedrock layer (22), and the technical casing (14) is arranged around the inner circumference of the second cement casing (13); When designing the position of the borehole (100), it is determined that the borehole (100) is a directional borehole (100), and the offset position of the borehole (100) is arranged perpendicular to the mining direction of the working face, or the position of the borehole (100) is arranged in the direction opposite to the mining direction of the working face.

7. The overburden separation grouting method according to claim 6, characterized in that: The pulp running prevention method further comprises: When a fault exists, analyzing the section of the borehole (100) affected by the fault, and if the section of the borehole (100) affected by the fault is in the bedrock layer (22) or below the bedrock layer (22), extending the borehole (100) below the bedrock layer (22), and setting a casing assembly (1) in the borehole (100) to isolate the section of the fault affected outside the technical casing (14); When a fault is present, the borehole (100) is extended above the affected section of the fault.

8. The overburden separation grouting method according to claim 6, characterized in that: The pulp running prevention method further comprises: When the casing assembly (1) is arranged in the borehole (100), a reserved section (15) is arranged at the lower end of the technical casing (14); the reserved section (15) is retractable relative to the technical casing (14) along the extension direction of the technical casing (14); when the lower end of the technical casing (14) receives ground stress, the reserved section (15) is extended to extend the technical casing (14); After the drilling (100) is completed, if it is analyzed that the drilling (100) does not meet the grouting conditions, a water pressure test is performed in the drilling (100), and if the orifice pressure is lower than the preset orifice pressure, the drilling (100) is blocked.

9. A method for treating slurry leakage, characterized in that: include: A method for treating slurry leakage in a well, wherein the method for treating slurry leakage in a well is the method for treating slurry leakage in a well as claimed in any one of claim 2, wherein when the water inflow is greater than the slurry leakage, the volume of cement slurry injected into the borehole (100) is 2 to 4 times the volume of the borehole (100), and the preset interval time is greater than 8 hours; A method for treating slurry on the ground, wherein the method for treating slurry on the ground is the method for treating slurry on the ground according to claim 3, wherein the preset interval time is greater than 12 hours, V 浆 =1.5~2V 清 .

10. The slurry running treatment method according to claim 9, characterized in that:When the slurry flow rate is greater than the water inflow rate, the volume of clean water containing the tracer injected into the borehole (100) is 4 to 6 times the volume of the borehole (100).

Citation Information

Cited By

  • Method for treating upper and lower water gushing and slurry gushing of separated layer grouting well through first blocking and then solidifying

    CN122630160A