Method for screening and baking battery cells with overproof water content based on formation process
Through multi-step charging and DQ/DV curve analysis of the synthesis process, combined with database screening, a lithium battery cell with excess moisture can be identified without disassembly, solving the problem of insufficient moisture detection in the existing technology and improving battery performance and security.
Patent Information
- Application Number
- CN202410879619.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-05
AI Technical Summary
The existing lithium battery baking process has limited number of random inspections, and it is impossible to effectively identify battery cells with excessive water content, resulting in damage to the battery cell's electrical performance and safety risks. It is difficult for the existing technology to identify and pick out battery cells with excessive moisture in advance.
Using a method based on the shaping process, the moisture content of the battery cell is controlled by adjusting the baking process and shaping equipment, multi-step charging and recording into data, and a characteristic value screen is established by using DQ/DV curve analysis and database to identify the moisture exceeding the standard. Battery cells can be identified in advance without disassembly.
Effectively screen out battery cells with excessive moisture, identify and select them in advance, avoid damage to the battery cell's electrical performance and safety risks, and improve the capacity and safety of the battery pack.
Smart Images

Figure CN118897207A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium battery detection, and in particular relates to a method for screening batteries with excessive baking water content based on a formation process. Background Art
[0002] The existing lithium battery baking process moisture detection has a limited number of random inspections and cannot represent the moisture content of the entire batch of battery cells, resulting in individual battery cells with excessive water content, or a small number of battery cells being stored for too long, resulting in excessive baking moisture content that cannot be identified and picked out, seriously affecting the battery cell's electrical performance. In other words, the disadvantage of the existing technology is that batteries with high baking moisture content cannot be selected, and batteries with high baking moisture content or even seriously exceeding the standard cannot be screened out. For cylindrical, square, and soft-pack battery cell systems, the cylindrical core is tightly pasted, and batteries with excessive moisture content will not bulge in the later stage, but there is a risk of continuous increase in internal pressure to reach the explosion-proof threshold. For square batteries with excessive moisture content, after capacity division, they will be affected by continuous gas production, and the electrode will rebound and there will be electrical problems. The problem of core bulging, etc., the soft pack phenomenon is similar to the square; in addition, in terms of electrical performance, the voltage, internal resistance, K value and other electrical performance data of the ultra-high water content battery cell are not significantly different from those of the normal battery cell. The uneven lithium insertion phenomenon and uneven black spots can only be seen by disassembling the full-charged battery to observe the interface of the negative electrode sheet, or by analyzing the capacity retention rate of the battery cell after cycling. This method has serious hysteresis. If it is paired with normal battery cells, it will greatly affect the capacity of the battery pack, the cycle will be greatly reduced, and there is a safety risk; therefore, it is very necessary to provide a method for identifying and picking out batteries with excessive water content in advance, using data analysis to identify, and without disassembling the battery cells, which is based on the formation process to screen and bake batteries with excessive water content. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and to provide a method for screening and baking batteries with excessive moisture content based on a formation process, which can identify and pick out batteries with excessive moisture in advance, use data analysis to identify, and do not need to disassemble the batteries.
[0004] The object of the present invention is achieved by: a method for screening and baking batteries with excessive water content based on a formation process, the method comprising the following steps:
[0005] Step 1: Cell preparation: adjust the baking process, control the moisture content after baking to 100, 180, and 300 ppm, and let it stand for a sufficient time after injection until the electrode is completely soaked;
[0006] Step 2: Connect the battery cell in step 1 to the formation equipment for formation: the first step is to charge to 3% SOC at 0.05C; the second step is to charge to 7.5% SOC at 0.1C; the third step is to charge to 30% SOC at 0.2C;
[0007] Step 3: The remaining processes flow normally, record the formation data, and obtain the formation curve;
[0008] Step 4: Analyze the specific data through the formation curve, compare the characteristic values of the first step charging capacity, voltage, the second step charging capacity, voltage, and set the lower limit of capacity and voltage to screen out unqualified cells;
[0009] Step 5: Database establishment: Establish a normal batch database to ensure that the quantity is greater than 5000pcs. In the subsequent screening process, normal batch cells can be gradually included in the database;
[0010] Step 6: If there is a change in the main material, the database of the materials with great impact should be re-established;
[0011] Step 7: Identify the charged capacity through the formation process, the voltage characteristic data at the end of charging, and compare it with a large number of normal data to select the battery cells with extremely high moisture content during baking.
[0012] The injection in step 1 is to inject the electrolyte containing VC additive, and the content of VC in the electrolyte is 1.2% to 4.8%.
[0013] The content of VC in the electrolyte is 2.2%.
[0014] The decomposition potential of the electrolyte additive VC is 0.6-1.2V, and the decomposition potential of water is 2V-2.2V.
[0015] The process setting for the formation in step 2 is specifically as follows: the SOC at the end of formation is set at 20%-40%; the first step is to charge 2%-5% of the capacity and the rate is 0.05C-0.1C; the second step is to charge 10%-20% of the capacity and the rate is 0.1C-0.3C.
[0016] The precision of the formation equipment in step 2 is specifically as follows: current precision: ±(0.05%RD+0.05%FS); time precision: resolution 1s, precision ±0.1%; voltage resolution: 0.1mV; current resolution: 0.1mA; data sampling time: 1s / time; sampling time deviation during the entire formation process is ≤0.3%.
[0017] The screening formula for screening out unqualified battery cells in step 4 is: if the baking moisture standard is controlled within 100ppm, the formation data of a large batch of data with a baking moisture of 100ppm is taken as a normal batch: the first step charging capacity curve is less than the normal batch average charging capacity and the second step charging capacity curve is less than the normal batch average charging capacity; the first step charging end voltage is less than the normal batch end voltage and the second step charging end voltage is less than the normal batch end voltage.
[0018] After the corresponding screening formula is used in step 4 to complete the screening of unqualified cells, some cells may be misjudged and need to be exported into detailed data. Then, the differential capacity curve obtained by data smoothing can be checked for obvious abnormal film formation peaks to screen out cells with water content that significantly exceeds the standard.
[0019] The main material changes in step 6 include positive electrode materials, negative electrode materials, copper foil, aluminum foil, separator, and electrolyte.
[0020] The beneficial effects of the present invention are as follows: the present invention is a method for screening out cells with excessive baked moisture content based on a formation process. During use, the present invention screens out cells with excessive moisture content through characteristics such as the formation charge end voltage and the end capacity; the present invention distinguishes between the additive VC (vinyl carbonate) and the water decomposition potential through DQ / DV curve analysis; the present invention establishes a database and characteristic value screening criteria; the present invention can screen out cells with excessive baked moisture content in the formation process and identify and select them in advance; the present invention can identify by performing data analysis without disassembling the cells; the present invention has the advantages of identifying and selecting cells with excessive moisture content in advance, using data analysis for identification, and not requiring disassembling the cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a voltage change diagram for different water decompositions of the present invention.
[0022] Figure 2 It is a schematic diagram of the DQ / DV curve of the first step of the formation of the present invention.
[0023] Figure 3 It is a schematic diagram of DQ / DV curve analysis of the present invention. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with the accompanying drawings.
[0025] Example 1
[0026] like Figure 1-3 As shown, a method for screening batteries with excessive baking water content based on a formation process, the method comprises the following steps:
[0027] Step 1: Cell preparation: adjust the baking process, control the moisture content after baking to 100, 180, and 300 ppm, and let it stand for a sufficient time after injection until the electrode is completely soaked;
[0028] Step 2: Connect the battery cell in step 1 to the formation equipment for formation: the first step is to charge to 3% SOC at 0.05C; the second step is to charge to 7.5% SOC at 0.1C; the third step is to charge to 30% SOC at 0.2C;
[0029] Step 3: The remaining processes flow normally, record the formation data, and obtain the formation curve;
[0030] Step 4: Analyze the specific data through the formation curve, compare the characteristic values of the first step charging capacity, voltage, the second step charging capacity, voltage, and set the lower limit of capacity and voltage to screen out unqualified cells;
[0031] Step 5: Database establishment: Establish a normal batch database to ensure that the quantity is greater than 5000pcs. In the subsequent screening process, normal batch cells can be gradually included in the database;
[0032] Step 6: If there is a change in the main material, the database of the materials with great impact should be re-established;
[0033] Step 7: Identify the charged capacity through the formation process, the voltage characteristic data at the end of charging, and compare it with a large number of normal data to select the battery cells with extremely high moisture content during baking.
[0034] In this embodiment, the principle of the present invention is explained as follows: ① During formation, if the water content in the battery cell is very high, the lithium salt reacts with water to produce a large amount of H+. Under the catalysis of H+, the additive VC (vinylene carbonate) in the electrolyte undergoes ring opening, self-polymerization reaction and rapid side reaction with the negative electrode, etc., consuming a large amount of the additive VC (vinylene carbonate) and forming a loose SEI film. On the formation differential capacity curve dQ / dV, the VC (vinylene carbonate) film-forming peak is significantly higher, and the higher the water content, the stronger the peak value;
[0035] ② The additive VC (vinyl carbonate) in the electrolyte forms a dense SEI film on the surface of the negative electrode, which significantly helps the cycle performance of the battery cell and the first coulomb efficiency. In the formation stage, the additive VC (vinyl carbonate) forms a film before the solvent EC (ethylene carbonate) and DEC (diethyl carbonate) to protect the negative electrode. Generally speaking, the content of the electrolyte additive VC (vinyl carbonate) is relatively small (1.2%-4.8%), and the platform of the formation curve and the differential capacitance dQ / dV peak are not obvious in the whole curve. The content of VC (vinyl carbonate) in the electrolyte is 1.2% to 4.8%, preferably 2.2%;
[0036] ③ During formation, the decomposition potential of the electrolyte additive VC (vinyl carbonate) is between 0.6 and 1.2 V, and the decomposition potential of water is around 2 V (it varies in different electrolyte formulations). In the first charging stage of formation, it only takes about 2 minutes from 0 V to 2 V. During the voltage boosting process, the additive VC (vinyl carbonate) has not yet completed its reaction, and water participates in the reaction, consuming the lithium ions deintercalated from the negative electrode. The lithium ions cannot be embedded in the negative electrode, resulting in a low positive electrode potential and a low open circuit voltage. The charging capacity in the first and second steps of formation will be low. Through data analysis, the differential capacity curve obtained shows that for cells with high baked moisture content, the film formation peak is significantly delayed.
[0037] In this embodiment, the present invention can also analyze the first coulombic efficiency. High water content consumes lithium ions deintercalated from the negative electrode, forming a loose SEI film and causing many side reactions, resulting in a low first coulombic efficiency, which can be identified by analyzing the first coulombic efficiency.
[0038] The present invention discloses a method for screening out cells with excessive baked water content based on a formation process. In use, the present invention screens out cells with excessive water content through characteristics such as the formation charge end voltage and the end capacity; the present invention distinguishes between additives VC (vinyl carbonate) and water decomposition potential through DQ / DV curve analysis; the present invention establishes a database and a characteristic value screening standard; the present invention can screen out cells with excessive baked water content in the formation process and identify and select them in advance; the present invention can identify cells by performing data analysis without disassembling the cells; the present invention has the advantages of identifying and selecting cells with excessive water content in advance, using data analysis for identification, and not requiring disassembling the cells.
[0039] Example 2
[0040] like Figure 1-3 As shown, a method for screening batteries with excessive baking water content based on a formation process, the method comprises the following steps:
[0041] Step 1: Cell preparation: adjust the baking process, control the moisture content after baking to 100, 180, and 300 ppm, and let it stand for a sufficient time after injection until the electrode is completely soaked;
[0042] Step 2: Connect the battery cell in step 1 to the formation equipment for formation: the first step is to charge to 3% SOC at 0.05C; the second step is to charge to 7.5% SOC at 0.1C; the third step is to charge to 30% SOC at 0.2C;
[0043] Step 3: The remaining processes flow normally, record the formation data, and obtain the formation curve;
[0044] Step 4: Analyze the specific data through the formation curve, compare the characteristic values of the first step charging capacity, voltage, the second step charging capacity, voltage, and set the lower limit of capacity and voltage to screen out unqualified cells;
[0045] Step 5: Database establishment: Establish a normal batch database to ensure that the quantity is greater than 5000pcs. In the subsequent screening process, normal batch cells can be gradually included in the database;
[0046] Step 6: If there is a change in the main material, the database of the materials with great impact should be re-established;
[0047] Step 7: Identify the charged capacity through the formation process, the voltage characteristic data at the end of charging, and compare it with a large number of normal data to select the battery cells with extremely high moisture content during baking.
[0048] The injection in step 1 is to inject the electrolyte containing VC additive, and the content of VC in the electrolyte is 1.2% to 4.8%.
[0049] The content of VC in the electrolyte is 2.2%.
[0050] The decomposition potential of the electrolyte additive VC is 0.6-1.2V, and the decomposition potential of water is 2V-2.2V.
[0051] The process setting for the formation in step 2 is specifically as follows: the SOC at the end of formation is set at 20%-40%; the first step is to charge 2%-5% of the capacity and the rate is 0.05C-0.1C; the second step is to charge 10%-20% of the capacity and the rate is 0.1C-0.3C.
[0052] In this embodiment, the setting of the formation process is related to whether normal and abnormal battery cells can be distinguished by characteristic values such as voltage, capacity, and differential capacity curve. The difference between battery cells with ultra-high moisture and normal battery cells is small after reaching the platform voltage, and they are difficult to identify. The formation process setting is mainly controlled to distinguish the characteristic values below the platform voltage; the platform voltage refers to the voltage value corresponding to the smallest voltage change and the largest capacity change, and batteries with different compositions are also different, for example: lithium iron phosphate: the platform voltage during charging is about 3.6V, and the platform voltage during discharging is about 3.2V.
[0053] The precision of the formation equipment in step 2 is specifically as follows: current precision: ±(0.05%RD+0.05%FS); time precision: resolution 1s, precision ±0.1%; voltage resolution: 0.1mV; current resolution: 0.1mA; data sampling time: 1s / time; the sampling time deviation during the entire formation process is ≤0.3%. The formation equipment needs to be calibrated regularly. Since the performance difference between normal and abnormal cells in formation is small, the equipment precision is required to be high.
[0054] The screening formula for screening out unqualified battery cells in step 4 is: if the baking moisture standard is controlled within 100ppm, the formation data of a large batch of data with a baking moisture of 100ppm is taken as a normal batch: the first step charging capacity curve is less than the normal batch average charging capacity and the second step charging capacity curve is less than the normal batch average charging capacity; the first step charging end voltage is less than the normal batch end voltage and the second step charging end voltage is less than the normal batch end voltage.
[0055] After the corresponding screening formula is used in step 4 to complete the screening of unqualified cells, some cells may be misjudged and need to be exported into detailed data. Then, the differential capacity curve obtained by data smoothing can be checked for obvious abnormal film formation peaks to screen out cells with water content that significantly exceeds the standard.
[0056] The main material changes in step 6 include positive electrode materials, negative electrode materials, copper foil, aluminum foil, separator, and electrolyte.
[0057] In this embodiment, if there is a change in the main material (positive electrode material, negative electrode material, copper foil, aluminum foil, diaphragm, electrolyte, etc.), the materials with great influence should re-establish the database. Different main materials will reflect different performances and there will be slight differences. The required data can be screened out through the process IMES system.
[0058] In this embodiment, the battery cell preparation: adjust the baking process, control the moisture after baking to 100, 180, and 300 ppm in sequence, let it stand for a sufficient time after injection until the electrode is completely wetted, and the formation process is carried out in 3 steps, the first step is 0.05C charging to 3% SOC, the second step is 0.1C charging to 7.5% SOC, and the third step is 0.2C charging to 30% SOC. The remaining processes flow normally, record the formation data, and obtain the following data;
[0059]
[0060] From the data, it can be concluded that the higher the moisture content, the lower the charging capacity in the first step, the lower the voltage at the end of the first step, and the smaller the difference in the data at the beginning of the second step. As the SOC increases, it becomes more difficult to distinguish after reaching the platform voltage. This is one of the reasons why cells with high moisture content are difficult to identify;
[0061] Notes: 1. Exclude other abnormal data; 2. Exclude factors affected by power outages due to abnormal equipment points; 3. The differential capacity curve interval is 5mv / s;
[0062] According to the above steps, we can get Figure 1-3,Figure analysis: In the comparison of voltage, the normal curve increases voltage quickly, and the higher the water content, the slower the voltage increase speed, which is consistent with the phenomenon of violent side reactions and low positive electrode potential; the higher the water content, the faster the power loss speed during the static process after the first step of charging is completed, indicating that the film formation effect is worse;
[0063] After the voltage curve comparison is completed, it is necessary to further confirm it through the differential capacity curve. Figure 2 The middle is the dQ / dV curve of the first step of formation charging, with the voltage of 100ppm as the horizontal axis for reference, and the vertical axis is the integral dQ / dV of capacity over voltage; due to the large difference in voltage data for different water content, Figure 3 It is not possible to use voltage as the horizontal axis for specific reference, and the vertical axis is the integral of capacity over voltage dQ / dV;
[0064] Depend on Figure 2 , 3 It can be seen that the VC (vinyl carbonate) film-forming peak of a normal battery cell is not obvious (related to the electrolyte formula). From the differential capacity curve, it can be seen that the higher the water content, the higher the film-forming peak value, which means that the side reaction is more intense and the film-forming peak value also has a certain lag. The second peak is the lithium insertion peak. Affected by water electrolysis, the higher the water content, the lower the peak value. The lithium insertion peak also lags, indicating that more side reactions are generated, more lithium ions participate in the formation of the SEI film, and form an uneven SEI film. In the corresponding electrochemical impedance spectrum, it is manifested as an increase in impedance in the low-frequency zone, and the corresponding AC internal resistance will increase, but it is not convenient to identify by the difference in internal resistance. The above screening steps can be used to pick out the battery cells with ultra-high water content.
[0065] The present invention discloses a method for screening out cells with excessive baked water content based on a formation process. In use, the present invention screens out cells with excessive water content through characteristics such as the formation charge end voltage and the end capacity; the present invention distinguishes between additives VC (vinyl carbonate) and water decomposition potential through DQ / DV curve analysis; the present invention establishes a database and a characteristic value screening standard; the present invention can screen out cells with excessive baked water content in the formation process and identify and select them in advance; the present invention can identify cells by performing data analysis without disassembling the cells; the present invention has the advantages of identifying and selecting cells with excessive water content in advance, using data analysis for identification, and not requiring disassembling the cells.
Claims
1. A method for screening batteries with excessive baking water content based on a formation process, characterized in that: The method comprises the following steps: Step 1: Cell preparation: adjust the baking process, control the moisture content after baking to 100, 180, and 300 ppm, and let it stand for a sufficient time after injection until the electrode is completely soaked; Step 2: Connect the battery cell in step 1 to the formation equipment for formation: the first step is to charge to 3% SOC at 0.05C; the second step is to charge to 7.5% SOC at 0.1C; the third step is to charge to 30% SOC at 0.2C; Step 3: The remaining processes flow normally, record the formation data, and obtain the formation curve; Step 4: Analyze the specific data through the formation curve, compare the characteristic values of the first step charging capacity, voltage, the second step charging capacity, voltage, and set the lower limit of capacity and voltage to screen out unqualified cells; Step 5: Database establishment: Establish a normal batch database to ensure that the quantity is greater than 5000pcs. In the subsequent screening process, normal batch cells can be gradually included in the database; Step 6: If there is a change in the main material, the database of the materials with great impact should be re-established; Step 7: Identify the charged capacity through the formation process, the voltage characteristic data at the end of charging, and compare it with a large number of normal data to select the battery cells with extremely high moisture content during baking.
2. A method for screening batteries with excessive baking water content based on a formation process according to claim 1, characterized in that: The injection in step 1 is to inject the electrolyte containing VC additive, and the content of VC in the electrolyte is 1.2%~4.8%.
3. A method for screening batteries with excessive baking water content based on a formation process according to claim 2, characterized in that: The content of VC in the electrolyte is 2.2%.
4. A method for screening batteries with excessive baking water content based on a formation process according to claim 3, characterized in that: The decomposition potential of the electrolyte additive VC is 0.6-1.2V, and the decomposition potential of water is 2V-2.2V.
5. The method for screening batteries with excessive baking water content based on a formation process according to claim 1, characterized in that: The process settings for the formation in step 2 are specifically as follows: the SOC at the end of formation is set at 20%-40%; the first step is to charge 2%-5% of the capacity and the rate is 0.05C-0.1C; the second step is to charge 10%-20% of the capacity at the rate of 0.1C-0.3C.
6. A method for screening batteries with excessive baking water content based on a formation process according to claim 5, characterized in that: The precision of the formation equipment in step 2 is specifically as follows: current precision: ±(0.05%RD+0.05%FS); time precision: resolution 1s, precision ±0.1%; voltage resolution: 0.1mV; current resolution: 0.1mA; data sampling time: 1s / time; sampling time deviation during the entire formation process is ≤0.3%.
7. A method for screening batteries with excessive baking water content based on a formation process according to claim 1, characterized in that: The screening formula for screening out unqualified battery cells in step 4 is: if the baking moisture standard is controlled within 100ppm, the formation data of a large batch of data with a baking moisture of 100ppm is taken as a normal batch: the first step charging capacity curve is less than the normal batch average charging capacity and the second step charging capacity curve is less than the normal batch average charging capacity; the first step charging end voltage is less than the normal batch end voltage and the second step charging end voltage is less than the normal batch end voltage.
8. A method for screening batteries with excessive baking water content based on a formation process according to claim 7, characterized in that: After the corresponding screening formula is used in step 4 to complete the screening of unqualified cells, some cells may be misjudged and need to be exported into detailed data. Then, the differential capacity curve obtained by data smoothing can be checked for obvious abnormal film formation peaks to screen out cells with water content that significantly exceeds the standard.
9. The method for screening out batteries with excessive baking water content based on a formation process according to claim 1, characterized in that: The main material changes in step 6 include positive electrode materials, negative electrode materials, copper foil, aluminum foil, separator, and electrolyte.
Citation Information
Cited By
Battery detection method, battery manufacturing process and battery
CN119738733A
Battery detection method, battery manufacturing process, and battery
CN119738733B
Formation method for improving cycling stability of silicon-containing soft package lithium ion battery
CN120376798A