Wet preparation process of electrode plate with self-supporting electrode plate and current collector integrally formed and electrode plate
By adding fibrosis process and solvent dispersion process to the wet preparation process of the battery electrode sheet, the firm connection between the self-supporting electrode sheet and the current collector and the uniform dispersion of the electrode active substances are achieved, and the uneven dispersion of the electrode active substances in the battery is solved. The problem of poor bonding improves the stability and cycle life of the battery.
Patent Information
- Application Number
- CN202410943854.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
In the production of existing self-supporting electrode sheets, it is difficult to achieve uniform dispersion of electrode active substances and firm connection with current collectors, affecting the stability and cycle life of the battery.
By using a wet preparation process of integrated molding of self-supporting electrode sheet and current collector, the electrode active substance, conductive agent and binder are mixed and fibrated, and stirred and dispersed with the solvent, it is directly coated on the current collector, and then baked. The electrode sheet is made by dry and cold pressing to form a self-supporting fiber network structure, solving the problems of uniform dispersion of electrode active substances and bonding to the current collector.
It improves the mechanical properties and conductivity of the electrode sheet, enhances the stability and cycle life of the battery, reduces internal resistance, and ensures uniform dispersion of the electrode active substance and firm connection with the current collector.
Smart Images

Figure CN118899172A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical fields of batteries, supercapacitors and capacitors, and in particular to a wet method preparation process of an electrode sheet in which a self-supporting electrode sheet and a current collector are integrally formed. Background Art
[0002] A self-supporting electrode sheet is an electrode sheet that does not require an additional current collector and relies on its own electrode material to complete mechanical support. The self-supporting structure is beneficial to improving the conductivity and mechanical stability of the electrode and extending the battery cycle life.
[0003] At present, the relatively economical and mainstream method for making self-supporting pole pieces is mainly to fiberize the electrode material and then extrude the electrode material to form a self-supporting pole piece, but this method faces some challenges, such as how to achieve uniform dispersion of electrode active materials. In addition, although the self-supporting pole piece does not require the current collector to rely on its own electrode material for mechanical support, it is still necessary to connect the self-supporting pole piece with the current collector in battery manufacturing to achieve external electrical circulation. How to connect the self-supporting pole piece with the current collector is also a current technical problem. Summary of the invention
[0004] The purpose of the present invention is to provide a wet method for preparing an electrode sheet in which a self-supporting electrode sheet and a current collector are integrated to solve the problems raised in the above background technology. To achieve the above purpose, the present invention provides the following technical solutions:
[0005] The first aspect of the present invention provides a wet method for preparing an electrode sheet in which a self-supporting electrode sheet and a current collector are integrally formed. The application fields include but are not limited to the fields of batteries, supercapacitors, and capacitors. The battery referred to below generally refers to lithium-ion batteries, sodium-ion batteries, supercapacitors, and capacitors. The wet method for preparing an electrode sheet comprises the following steps:
[0006] The electrode active material, the conductive agent and the binder are uniformly mixed to obtain a mixture I;
[0007] Fiberizing the mixture I to obtain a fiberized mixture II;
[0008] The solvent and the fiberized mixture II are stirred and dispersed uniformly to obtain a liquid mixture III;
[0009] The liquid mixture III is coated on the current collector, and the finished electrode sheet is obtained through drying and cold pressing.
[0010] Furthermore, the mass percentage of the electrode active material in the mixture I is 80-98.5%.
[0011] Furthermore, the electrode active material includes a positive electrode active material, and the positive electrode active material includes one or more of activated carbon, lithium iron phosphate, lithium nickel cobalt manganese oxide and lithium cobalt oxide.
[0012] Furthermore, the electrode active material includes a negative electrode active material, and the negative electrode active material includes one or more of artificial graphite, natural graphite, mesophase carbon microspheres, activated carbon, hard carbon, soft carbon, lithium titanate, silicon carbon and silicon-tin alloy.
[0013] Furthermore, the mass percentage of the conductive agent in the mixture I is 0.5-10%.
[0014] Furthermore, the conductive agent includes one or more of conductive carbon black, acetylene black, graphene, conductive graphite, conductive carbon tube and conductive carbon fiber.
[0015] Furthermore, the mass percentage of the conductive binder in the mixture I is 1 to 10%.
[0016] Furthermore, the binder includes one or more of SBR, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride and sodium carboxymethyl cellulose.
[0017] Furthermore, the method of fiberizing the mixture I includes one or more of air flow milling, high-speed stirring, mechanical milling, shear stirring and internal mixing.
[0018] Furthermore, the solvent includes one or more of acetone, NMP, ethanol and pure water.
[0019] Furthermore, the liquid mixture III is applied by rolling or spraying.
[0020] Furthermore, the current collector is one of aluminum foil, copper foil and stainless steel foil.
[0021] A second aspect of the present invention provides an electrode sheet formed by integrating a self-supporting electrode sheet and a current collector, wherein the electrode sheet is produced by any of the wet preparation processes described above.
[0022] The beneficial effects of the present invention are:
[0023] 1. Compared with the traditional wet process, the present invention innovatively adds a fiberization process. By mixing the electrode active material, the conductive agent and the binder evenly and then fiberizing them, the electrode layer after the electrode sheet is formed forms a self-supporting fiber network structure. The electrode sheet is not easy to fall off and is more firmly bonded to the current collector, thereby reducing the internal resistance of the electrode sheet. Compared with the traditional wet process electrode sheet, it can have better mechanical properties and conductive properties;
[0024] 2. Compared with the traditional dry method of making pole pieces by directly extruding the fiberized material into pole pieces, the present invention uses a solvent to stir and disperse the fiberized mixture II evenly, and then directly applies the liquid mixture III on the current collector, so that the electrode active material is dispersed more evenly and the electrode pieces are more uniform, which is beneficial to improving the stability of the battery and solves the technical problem of bonding the dry pole piece to the current collector. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 The figure is a flow chart of the wet preparation process of the present invention.
[0027] Figure 2 Schematic diagram of the fiberized mixture II prepared in the present invention.
[0028] Figure 3 This is a schematic diagram of a finished electrode sheet produced by the present invention.
[0029] It should be noted that the drawings are not necessarily drawn to scale, but are merely shown in a schematic manner that does not affect the reader's understanding. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0032] It should be further understood that the term "and / or" used in the present description and the appended claims refers to and includes any and all possible combinations of one or more of the associated listed items.
[0033] The first aspect of the present application provides a wet method for preparing an electrode sheet in which a self-supporting electrode sheet and a current collector are integrated, which is used to prepare a positive electrode sheet and a negative electrode sheet. The application fields include but are not limited to batteries, supercapacitors, and capacitors. The battery referred to below generally refers to lithium-ion batteries, sodium-ion batteries, supercapacitors, and capacitors. Figure 1 The wet preparation process of the electrode sheet includes the following steps:
[0034] S1. Mix and stir 80-98.5% of electrode active material, 0.5-10% of conductive agent, and 1-10% of binder by mass percentage to obtain mixture I. It should be noted that when preparing positive electrode sheets, the electrode active material needs to use the corresponding positive electrode active material, and the positive electrode active material can use all known positive electrode active materials in the prior art, such as: activated carbon, lithium iron phosphate, lithium nickel cobalt manganese oxide and lithium cobalt oxide. Similarly, when preparing negative electrode sheets, the electrode active material needs to use the corresponding negative electrode active material, and the negative electrode active material can use all known negative electrode active materials in the prior art, such as: artificial graphite, natural graphite, mesophase carbon microspheres, activated carbon, hard carbon, soft carbon, lithium titanate, silicon carbon and silicon tin alloy. Conductive agents can use all known conductive agents in the prior art, such as: one or more of conductive carbon black, acetylene black, graphene, conductive graphite, conductive carbon tubes and conductive carbon fibers. The binder may be any known binder in the prior art, such as one or more of SBR, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride and sodium carboxymethyl cellulose.
[0035] S2. Fiberize the mixture I to obtain a fiberized mixture II. Figure 2 , which enables the electrode layer after the electrode sheet is formed to form a self-supporting fiber network structure. Compared with the traditional wet-process electrode sheet, the electrode sheet prepared in this embodiment has better mechanical properties and conductive properties. It should be noted that the method for fiberizing the mixture I can use all known fiberizing methods in the prior art, such as: one or more of air flow milling, high-speed stirring, mechanical milling, shear stirring and banburying.
[0036] S3, mixing the solvent and the fiberized mixture II, using the solvent to disperse and dissolve the fiberized mixture II into a liquid state, fully stirring and dispersing it evenly through a mixer and a high-speed disperser, to obtain a liquid mixture III, which is conveniently and evenly coated on the current collector, and can make the mainstream self-supporting pole piece electrode active material evenly dispersed, which to a certain extent solves the problem of uniform dispersion of the mainstream self-supporting pole piece electrode material. It should be noted that the solvent can use all known solvents in the prior art, such as: one or more of acetone, NMP, ethanol and pure water.
[0037] S4. The stirred and dispersed liquid mixture III is directly coated on the current collector by roller coating or spraying, thereby avoiding the problem of connecting the self-supporting electrode sheet with the current collector, which is beneficial to improving the stability of the battery; after uniform coating, it is baked and dried to remove the solvent and moisture absorbed in the air, and then cold-pressed using a rolling device to obtain a finished electrode sheet after drying, see Figure 3 It should be noted that the current collector can be made of one of aluminum foil, copper foil and stainless steel foil.
[0038] The advantages of this application are:
[0039] 1. Compared with the traditional wet process, the present invention innovatively adds a fiberization process. By mixing the electrode active material, the conductive agent and the binder evenly and then fiberizing them, the electrode layer after the electrode sheet is formed forms a self-supporting fiber network structure. The electrode sheet is not easy to fall off and is more firmly bonded to the current collector, thereby reducing the internal resistance of the electrode sheet. Compared with the traditional wet process electrode sheet, it can have better mechanical properties and conductive properties;
[0040] 2. Compared with the traditional dry method of making electrodes by directly extruding fiberized materials into electrodes, the present invention uses a solvent to stir and disperse the fiberized mixture II evenly, and then directly applies the liquid mixture III on the current collector, so that the electrode active material is dispersed more evenly, making the electrode sheet more uniform, which is beneficial to improving the stability of the battery and solving the technical problem of bonding the dry electrode sheet to the current collector.
[0041] Embodiment 1:
[0042] This embodiment provides a wet method for preparing a positive electrode sheet in which a self-supporting electrode sheet and a current collector are integrally formed, and the steps are as follows:
[0043] First, the positive electrode active material, conductive agent and binder (polytetrafluoroethylene) are put into a V-type mixer and stirred evenly, wherein the weight ratio of the positive electrode active material, conductive agent and binder is 97.5:1.0:1.5; then the mixture of the positive electrode active material, conductive agent and binder (polytetrafluoroethylene) stirred evenly is subjected to air flow mill fiberization; then, an appropriate amount of NMP solvent is added to the fiberized mixture, and the mixture is fully stirred and dispersed evenly in a planetary mixer to obtain a slurry; the obtained slurry is then coated on the collector by roller coating, and the positive electrode coating surface density is 60 mg / cm2; finally, the solvent and moisture absorbed in the air are removed by baking and drying, and after the electrode sheet is dried, the electrode sheet is cold pressed using a rolling equipment to obtain a finished positive electrode sheet.
[0044] Embodiment 2:
[0045] This embodiment provides a wet method for preparing a negative electrode sheet in which a self-supporting electrode sheet and a current collector are integrally formed, and the steps are as follows:
[0046] First, the negative electrode active material, conductive agent and binder (polytetrafluoroethylene) are put into a V-type mixer and stirred evenly, wherein the weight ratio of the negative electrode active material, conductive agent and binder is 96.0:1.0:3.0; then the stirred evenly stirred mixture of the negative electrode active material, conductive agent and binder (polytetrafluoroethylene) is subjected to air flow mill fiberization; then, an appropriate amount of NMP solvent is added to the fiberized mixture, and the mixture is fully stirred and dispersed evenly in a planetary mixer to obtain a slurry; the obtained slurry is then coated on the collector by roller coating, and the negative electrode coating surface density is 38 mg / cm2; finally, the solvent and moisture absorbed in the air are removed by baking and drying, and after the electrode sheet is dried, the electrode sheet is cold pressed using a rolling equipment to obtain a finished negative electrode sheet.
[0047] Comparative Example 1:
[0048] The steps for preparing the positive electrode sheet in this comparative example are as follows:
[0049] First, the positive electrode active material, conductive agent and binder (polytetrafluoroethylene) are put into a V-type mixer and stirred evenly, wherein the weight ratio of the positive electrode active material, conductive agent and binder is 97.5:1.0:1.5; then, an appropriate amount of NMP solvent is added to the evenly stirred mixture of the positive electrode active material, conductive agent and binder (polytetrafluoroethylene), and the mixture is fully stirred and dispersed evenly in a planetary mixer to obtain a slurry; then, the prepared slurry is coated on the current collector by roller coating, and the positive electrode coating surface density is 60 mg / cm2; finally, the solvent and moisture absorbed in the air are removed by baking and drying, and after the electrode sheet is dried, the electrode sheet is cold pressed using a rolling equipment to obtain a finished positive electrode sheet.
[0050] Comparative Example 2:
[0051] The steps of preparing the negative electrode sheet in this comparative example are as follows:
[0052] First, the negative electrode active material, conductive agent, and binder (polytetrafluoroethylene) are put into a V-type mixer and stirred evenly, wherein the weight ratio of the negative electrode active material, conductive agent, and binder is 96.0:1.0:3.0; then, an appropriate amount of NMP solvent is added to the evenly stirred mixture of the positive electrode active material, conductive agent, and binder (polytetrafluoroethylene), and the mixture is fully stirred and dispersed evenly in a planetary mixer to obtain a slurry; then, the prepared slurry is coated on the collector by roller coating, and the negative electrode coating surface density is 38 mg / cm2; finally, the solvent and moisture absorbed in the air are removed by baking and drying, and after the electrode sheet is dried, the electrode sheet is cold pressed using a rolling equipment to obtain a finished negative electrode sheet.
[0053] Conductivity test:
[0054] To ensure that the electrode sheets of Example 1 and Example 2 and the electrode sheets of Comparative Example 1 and Comparative Example 2 are under specific surface density conditions, the conductivity of each electrode sheet is tested using a conductivity tester, as shown in the following table:
[0055] Area density (mg / cm2) Conductivity(s / cm) Example 1 Positive electrode sheet 62 0.52 Example 2 Negative electrode sheet 40 9.65 Comparative Example 1 Positive Electrode Sheet 62 0.38 Comparative Example 2 Negative Electrode Sheet 40 8.83
[0056] Test result analysis:
[0057] According to the data analysis in the above table, under the same material and surface density conditions, the electrode sheet prepared by the wet preparation process of the present invention has a higher conductivity; the higher the conductivity of the electrode sheet, the lower the internal resistance of the manufactured battery, the lower the internal resistance and the less heat generated, and thus the longer the battery life; at the same time, the higher conductivity also proves that the bonding effect between the electrode active material and the current collector is better, that is, the problem of uniform dispersion of the electrode active material is solved.
[0058] Electrical performance test:
[0059] The four electrode sheets of Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were paired in pairs to make four groups of laminated structure experimental batteries. The internal resistance of each group of experimental battery samples was tested by an AC internal resistance tester, and each group of experimental battery samples was tested by a battery charge and discharge tester to obtain the room temperature discharge capacity, standard cycle life (normal temperature and humidity 1C / 500 cycles (%)), cycle life under double 85 conditions (85℃85RH%1C / 500 cycles (%)), and electrical performance data of 5C constant current charge ratio of each group of experimental battery samples, as shown in the following table:
[0060]
[0061]
[0062] Test result analysis:
[0063] According to the analysis of the data in the above table, it can be seen that the battery made of the electrode sheets prepared in Example 1 and Example 2 has a smaller internal resistance, a better cycle life, and a better high-temperature performance.
[0064] Regarding the embodiments of the present invention, it should also be noted that, in the absence of conflict, the embodiments of the present invention and the features therein may be combined with each other to obtain new embodiments.
[0065] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. The protection scope of the present invention shall be subject to the protection scope of the claims. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical content disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A wet method for preparing an electrode sheet with a self-supporting electrode sheet and a current collector integrated therein, characterized in that: The following steps are involved: The electrode active material, the conductive agent and the binder are uniformly mixed to obtain a mixture I; Fiberizing the mixture I to obtain a fiberized mixture II; The solvent and the fiberized mixture II are stirred and dispersed uniformly to obtain a liquid mixture III; The liquid mixture III is coated on the current collector, and the finished electrode sheet is obtained through drying and cold pressing.
2. The wet preparation process according to claim 1, characterized in that: The mass percentage of the electrode active material in the mixture I is 80-98.5%.
3. The wet preparation process according to claim 2, characterized in that: The electrode active material includes a positive electrode active material, and the positive electrode active material includes one or more of activated carbon, lithium iron phosphate, lithium nickel cobalt manganese oxide and lithium cobalt oxide.
4. The wet preparation process according to claim 2, characterized in that: The electrode active material includes a negative electrode active material, and the negative electrode active material includes one or more of artificial graphite, natural graphite, mesophase carbon microspheres, activated carbon, hard carbon, soft carbon, lithium titanate, silicon carbon and silicon-tin alloy.
5. The wet preparation process according to claim 1, characterized in that: The mass percentage of the conductive agent in the mixture I is 0.5-10%.
6. The wet preparation process according to claim 5, characterized in that: The conductive agent includes one or more of conductive carbon black, acetylene black, graphene, conductive graphite, conductive carbon tube and conductive carbon fiber.
7. The wet preparation process according to claim 1, characterized in that: The mass percentage of the conductive binder in the mixture I is 1-10%.
8. The wet preparation process according to claim 7, characterized in that: The binder includes one or more of SBR, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride and sodium carboxymethyl cellulose.
9. The wet preparation process according to claim 1, characterized in that: The fiberization method of the mixture I includes one or more of air flow milling, high-speed stirring, mechanical milling, shear stirring and internal mixing.
10. The wet preparation process according to claim 1, characterized in that: The solvent includes one or more of acetone, NMP, ethanol and pure water.
11. The wet preparation process according to claim 1, characterized in that: The liquid mixture III is applied by rolling or spraying.
12. The wet preparation process according to claim 1, characterized in that: The current collector is one of aluminum foil, copper foil and stainless steel foil.
13. An electrode sheet formed by integrating a self-supporting electrode sheet and a current collector, characterized in that: The electrode sheet is prepared by the wet preparation process according to any one of claims 1 to 12.