CoPt-coated NCNF electrode, preparation method thereof and lithium-carbon dioxide battery

Through the CoPt@NCNF electrode, a nitrogen-doped carbon nanofiber membrane-carrying cobalt-platinum alloy is used to promote carbon monoxide desorption, solving the problem of high charging potential of lithium-carbon dioxide batteries, and achieving efficient discharge of the battery and longer cycle life.

CN118899458APending Publication Date: 2024-11-05XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975712.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The charging potential of lithium-carbon dioxide batteries is high, resulting in slow reaction kinetics and limited mass transfer, which affects the cycle life and energy efficiency of the battery. It is difficult for existing catalysts to reduce the charging potential, especially carbon monoxide as the main discharge product.

Method used

CoPt@NCNF electrode is used to carry cobalt-platinum alloy through nitrogen-doped carbon nanofiber membrane, and the d-band center of platinum is adjusted by cobalt to promote desorption of carbon monoxide, reduce the charging potential, and realize carbon monoxide as the main discharge product.

Benefits of technology

Effectively reduce the charging potential of lithium-carbon dioxide batteries below 3.0V, improve reaction kinetics, broaden the application direction of batteries, and lay the foundation for commercialization and industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954461640000101
    Figure BDA0004954461640000101
  • Figure BDA0004954461640000102
    Figure BDA0004954461640000102
  • Figure HDA0004954461650000011
    Figure HDA0004954461650000011
Patent Text Reader

Abstract

The invention provides a CoPt-coated NCNF electrode, a preparation method of the CoPt-coated NCNF electrode and a lithium-carbon dioxide battery. The CoPt-coated NCNF electrode comprises a nitrogen-doped carbon nanofiber membrane and cobalt-platinum alloy loaded on the nitrogen-doped carbon nanofiber membrane. The center of a d band of platinum is adjusted and optimized by using transition metal cobalt, so that when the electrode is used as a positive electrode of a lithium-carbon dioxide battery, desorption of carbon monoxide serving as a reaction intermediate of the lithium-carbon dioxide battery can be promoted, and the lithium-carbon dioxide battery based on the CoPt-coated NCNF electrode takes carbon monoxide as a main discharge product, so that the lithium-carbon dioxide battery can be used for preparing the lithium-carbon dioxide battery with the CoPt-coated NCNF electrode. The charging potential of the battery is effectively reduced, and the charging potential is lower than 3.0 V.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium-carbon dioxide batteries, and in particular relates to a CoPt@NCNF electrode and a preparation method thereof, and a lithium-carbon dioxide battery. Background Art

[0002] Lithium-carbon dioxide batteries use carbon dioxide as the working gas. During battery operation, they can not only store and utilize carbon dioxide, but also have a theoretical energy density of 1876Wh kg -1 (far exceeding the current lithium-ion battery 387Wh kg -1 energy density), and has a very competitive advantage in the next generation of high energy density and high power density secondary energy storage devices. In addition, based on the energy storage needs of special environments such as the surface carbon dioxide concentration of Mars, which accounts for up to 96%, and the deep sea, which is oxygen-poor and carbon dioxide-rich, this novel battery has also shown great development and application prospects in the military and aerospace fields. Although lithium-carbon dioxide batteries have so many advantages, their positive electrode discharge products are currently lithium carbonate and carbon. On the one hand, lithium carbonate is a compound with a wide band gap and extremely low conductivity, and it is difficult to reversibly decompose electrochemically; on the other hand, both discharge products are solid, resulting in limited mass transfer and slow reaction kinetics during charging. Ultimately, the battery must complete a reversible cycle at a higher charging potential, but an excessively high charging potential not only affects the energy efficiency of the battery, but also causes side reactions such as the decomposition of the electrolyte, limiting the service life of the electrolyte and the lithium metal negative electrode, and ultimately resulting in a serious limitation in the number of battery cycles. This is also the core issue that currently restricts the rapid development of lithium-carbon dioxide batteries.

[0003] In response to the problem of difficulty in charging lithium-carbon dioxide batteries, scientific researchers have conducted a lot of exploration and research starting from the positive electrode catalyst. Compared with non-metallic or transition metal compounds, precious metals such as platinum, iridium, and ruthenium show excellent catalytic activity in lithium-carbon dioxide batteries due to their unique electronic configuration and high chemical stability, which can promote the battery's charging potential to drop below 4.0V, but it is still difficult to break through the 3.8V barrier. With the continuous advancement of research, some studies have pointed out that some molybdenum-based catalysts can stabilize lithium oxalate intermediates, making them the main discharge product and thus reducing the battery's charging potential, but they still cannot reduce the battery's charging potential to below 3.3V. In addition, lithium-carbon dioxide batteries based on the lithium oxalate mechanism, because the catalyst needs to participate in stabilizing the structure of lithium oxalate, cause irreversible reconstruction of the catalytic site, and ultimately lead to the battery cycle life based on this reaction process is generally very limited, most of which are even less than the cycle life based on the lithium carbonate and carbon reaction process. Therefore, it is difficult to further reduce the charging potential of lithium-carbon dioxide batteries by continuing to optimize the existing catalytic process, and exploring new charging and discharging processes is an inevitable choice at present.

[0004] Carbon monoxide is a possible intermediate in the reduction of carbon dioxide. Compared with carbon, the main reduction product at present, carbon monoxide as the final reduction product has at least the following three advantages: 1) The oxygen atom in the carbon monoxide molecule carries a partial negative charge, while the carbon atom carries a partial positive charge, so it has a chemical bond that is more easily oxidized than carbon. The presence of this polar bond causes carbon monoxide to be more easily oxidized than carbon. 2) The oxygen atom in carbon monoxide has a relatively high electron affinity, that is, it is easier to accept additional electrons to form adsorbed carbon monoxide. Although carbon atoms also have a certain electron affinity, their outer layer belongs to a 4-electron half-full state and has lower activity. Therefore, carbon monoxide molecules are more likely to accept electrons under electrochemical conditions. 3) Carbon monoxide molecules have high diffusion and migration activity, which can effectively promote mass transfer and ensure rapid reaction on the electrode surface. In contrast, pure carbon does not have this advantage. However, how to realize lithium-carbon dioxide batteries based on carbon monoxide as the main discharge product is currently a major problem. Summary of the invention

[0005] The object of the present invention is to provide a CoPt@NCNF electrode and a preparation method thereof and a lithium-carbon dioxide battery. The lithium-carbon dioxide battery based on the CoPt@NCNF electrode uses carbon monoxide as the main discharge product, which effectively reduces the charging potential of the battery, and the charging potential is lower than 3.0V.

[0006] The present invention is achieved through the following technical solutions:

[0007] The invention provides a CoPt@NCNF electrode, which comprises a nitrogen-doped carbon nanofiber membrane and a cobalt-platinum alloy loaded on the nitrogen-doped carbon nanofiber membrane.

[0008] Preferably, the molar ratio of cobalt to platinum in the cobalt-platinum alloy is (0.1-0.3):(0.5-3).

[0009] The present invention provides a method for preparing the CoPt@NCNF electrode, comprising:

[0010] S1, adding the nitrogen-doped carbon nanofiber membrane into an aqueous solution of chloroplatinic acid and cobalt chloride, immersing the membrane under stirring, and then freeze-drying the nitrogen-doped carbon nanofiber membrane;

[0011] S2, heat treating the freeze-dried nitrogen-doped carbon nanofiber membrane in a mixture of inert gas and hydrogen at 300-700° C. to obtain the CoPt@NCNF electrode.

[0012] Preferably, in S1, the method for preparing the nitrogen-doped carbon nanofiber membrane comprises:

[0013] (1) adding polyacrylonitrile and polyvinyl pyrrolidone into N,N-dimethylformamide and stirring to obtain an electrospinning precursor solution;

[0014] (2) The electrospinning precursor solution is electrospinned to obtain a polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane; the mass ratio of polyacrylonitrile, polyvinyl pyrrolidone and N,N-dimethylformamide is (1.0-1.4):0.5:(8-12);

[0015] (3) drying the polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane and pre-oxidizing it at 200-280° C.;

[0016] (4) The pre-oxidized polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane is carbonized in a protective atmosphere to obtain a nitrogen-doped carbon nanofiber membrane.

[0017] Preferably, in S1, in the aqueous solution, the concentration of chloroplatinic acid is 0.1-0.3M, and the concentration of cobalt chloride is 0.5-3M.

[0018] Preferably, in S1, the immersion time is 10-60 min.

[0019] Preferably, in S2, the heat treatment time is 1-4h.

[0020] The present invention provides a lithium-carbon dioxide battery, comprising a positive electrode, a separator and a negative electrode; the separator is located between the positive electrode and the negative electrode, and the positive electrode is the CoPt@NCNF electrode as described above.

[0021] Preferably, the diaphragm is glass fiber, polyimide, polyvinylidene fluoride-hexafluoropropylene or cellulose.

[0022] Preferably, the diaphragm is filled with an electrolyte, and the electrolyte is a dimethyl sulfoxide solution of lithium perchlorate, a dimethyl sulfoxide solution of lithium bis(trifluoromethylsulfonyl imide), a triethylene glycol dimethyl ether solution of lithium bis(trifluoromethylsulfonyl imide), or a tetraethylene glycol dimethyl ether solution of lithium bis(trifluoromethylsulfonyl imide.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention uses a nitrogen-doped carbon nanofiber membrane as a substrate, selects a platinum-based catalyst with excellent catalytic activity for lithium carbonate as a starting point, and uses transition metal cobalt to adjust and optimize the d-band center of platinum, so that when the electrode is used as the positive electrode of a lithium-carbon dioxide battery, it can promote the desorption of carbon monoxide, an intermediate of the lithium-carbon dioxide battery reaction, and then obtain a lithium-carbon dioxide battery with carbon monoxide as the main discharge product. Carbon monoxide as the main discharge product has faster reaction kinetics than the previous energy storage mechanism based on lithium carbonate plus carbon and based on lithium oxalate as the discharge product, and can effectively reduce the charging potential of the battery, achieving the goal of the battery potential being lower than 3V. The electrode of the present invention is a self-supporting electrode, which can be directly used in a lithium-carbon dioxide battery, reduces the electrode coating and preparation process, avoids the use of a binder and conductive carbon black, and can effectively reduce the side reactions in the battery charging and discharging process and the production cost of the battery.

[0025] The present invention uses nitrogen-rich sites of nitrogen-doped carbon nanofiber membranes as three-dimensional self-supporting substrates, then uses nitrogen sites to fix metal ions by impregnation, and finally calcines to successfully prepare CoPt@NCNF electrodes loaded with cobalt-platinum alloy on nitrogen-doped carbon nanofiber membranes. The preparation process and technology of the present invention are simple, and it is easy to achieve large-scale production, which has positive significance for the commercialization of lithium-carbon dioxide batteries.

[0026] Furthermore, the present invention constructs a nitrogen-rich three-dimensional self-supporting carbon substrate with fast mass transfer channels for the CoPt@NCNF electrode by optimizing the concentration of the electrospinning ink and the pre-oxidation temperature.

[0027] The lithium-carbon dioxide battery provided by the present invention uses CoPt@NCNF electrode as the positive electrode. Compared with Pt nanoparticles, after CoPt is alloyed, the interplanar spacing is compressed. This lattice strain can adjust the d-band center of Pt to move downward, thereby promoting the desorption of the reaction intermediate carbon monoxide on the Pt surface, so that the lithium-carbon dioxide battery uses carbon monoxide as the main discharge product, effectively reducing the battery's charging potential, which is lower than 3.0 V. This breakthrough can effectively broaden the research direction of lithium-carbon dioxide batteries and lay a solid foundation for the commercialization and industrial promotion of lithium-carbon dioxide batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1This is a scanning electron microscope image of the CoPt@NCNF self-supporting catalytic cathode in Example 1;

[0030] Figure 2 X-ray diffraction patterns of the CoPt@NCNF self-supporting catalytic positive electrode in Example 1 and the Pt@NCNF self-supporting catalytic positive electrode in Comparative Example 1;

[0031] Figure 3 This is a high-angle annular dark-field scanning transmission electron microscopy image of Pt alloy nanoparticles in the Pt@NCNF catalytic positive electrode in Comparative Example 1;

[0032] Figure 4 This is a high-angle annular dark-field scanning transmission electron microscopy image of CoPt alloy nanoparticles in the CoPt@NCNF catalytic positive electrode in Example 1;

[0033] Figure 5 20 μA cm for lithium-carbon dioxide batteries based on the catalytic positive electrodes of Example 1 CoPt@NCNF, Comparative Example 1 Pt@NCNF and Comparative Example 2 Co@NCNF -2 Current density, 100μAh cm -2 Comparison of discharge-charge performance at cut-off capacity;

[0034] Figure 6 The lithium-carbon dioxide battery in Example 1 at 50 μA cm -2 Current density, 500 μAh cm -2 Scanning electron microscopy images of the CoPt@NCNF catalytic cathode after discharge and charge at cut-off capacity;

[0035] Figure 7 The lithium-carbon dioxide battery in Example 1 at 50 μA cm -2 Current density, 500 μAh cm -2 X-ray diffraction patterns of CoPt@NCNF catalytic cathode before discharge, after discharge, and after charge at cut-off capacity;

[0036] Figure 8 The results of the positive electrode lithium-carbon dioxide battery based on CoPt@NCNF in Example 1, Pt@NCNF in Comparative Example 1 and Co@NCNF in Comparative Example 2 were shown in Figure 2 at 50 μA cm -2 Current density, 500 μAh cm -2 Gas phase mass spectrum of gas phase products after discharge at cut-off capacity;

[0037] Fig. 9 Schematic diagram of the structure of the lithium-carbon dioxide battery that can be charged at 3.0V in Example 7. DETAILED DESCRIPTION

[0038] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0039] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0040] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0041] The CoPt@NCNF electrode provided by the present invention comprises a nitrogen-doped carbon nanofiber membrane and a cobalt-platinum alloy supported on the nitrogen-doped carbon nanofiber membrane, wherein the molar ratio of cobalt to platinum in the cobalt-platinum alloy is preferably (0.1-0.3): (0.5-3).

[0042] In the present invention, the preparation method and steps of the CoPt@NCNF electrode are as follows:

[0043] a) Adding polyacrylonitrile and polyvinyl pyrrolidone into N,N-dimethylformamide, stirring at 40-60° C., and obtaining a precursor solution for electrospinning.

[0044] b) taking a certain amount of the electrospinning precursor liquid in a) into a needle tube, and obtaining a polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane by an electrospinning method.

[0045] c) drying the polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane in b) in a vacuum oven.

[0046] d) The polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane dried in c) is subjected to a pre-oxidation treatment in a muffle furnace at 200-280°C.

[0047] e) carbonizing the pre-oxidized polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane in d) in a protective atmosphere to obtain a nitrogen-doped carbon nanofiber membrane.

[0048] f) The nitrogen-doped carbon nanofiber membrane obtained in e) is placed in a culture dish, a certain amount of 0.1-0.3M chloroplatinic acid and 0.5-3M cobalt chloride aqueous solution is added, and the mixture is immersed in a stirring state for 10-60 minutes, and then the nitrogen-doped carbon nanofiber membrane is placed in liquid nitrogen for rapid freezing, and then freeze-dried.

[0049] g) The freeze-dried nitrogen-doped carbon nanofiber membrane in f) is heat treated in a mixture of argon and hydrogen at a heating rate of 2-5°C / min at 300-700°C for 1-4h to obtain a CoPt@NCNF electrode.

[0050] In step a), the mass ratio of polyacrylonitrile, polyvinyl pyrrolidone and N,N-dimethylformamide is: (1.0-1.4):0.5:(8-12).

[0051] The lithium-carbon dioxide battery based on the above-mentioned CoPt@NCNF electrode can achieve a charging potential lower than 3.0V. The specific composition of the lithium-carbon dioxide battery is as follows: the CoPt@NCNF electrode is used as the positive electrode, the porous membrane is used as the separator; the organic solvent containing lithium salt is used as the electrolyte; and metallic lithium is used as the negative electrode.

[0052] In the present invention, the diaphragm is a glass fiber diaphragm, a polyimide diaphragm, a polyvinylidene fluoride-hexafluoropropylene diaphragm, a cellulose diaphragm, etc.

[0053] In the present invention, the electrolyte is lithium perchlorate / dimethyl sulfoxide, lithium bis(trifluoromethylsulfonyl imide) / dimethyl sulfoxide, lithium bis(trifluoromethylsulfonyl imide) / triethylene glycol dimethyl ether or lithium bis(trifluoromethylsulfonyl imide) / tetraethylene glycol dimethyl ether.

[0054] In the present invention, the assembly steps of the lithium-carbon dioxide battery are: placing the positive electrode battery shell, CoPt@NCNF positive electrode, separator, electrolyte, negative electrode, current collector, negative electrode battery shell in sequence, and then encapsulating the battery.

[0055] The following will be described in detail with reference to the embodiments of the present invention. This embodiment is a preferred embodiment of the present invention and should not be used to limit the scope of the present invention. In the following examples, the methods and experimental equipment used are conventional methods and instruments unless otherwise specified. The experimental instruments used in the examples include a field emission scanning electron microscope (GeminiSEM 500), an X-ray diffractometer (Bruker D8 ADVANC), a double spherical aberration corrected transmission electron microscope (JEM-ARM300F2), a gas chromatograph (Agilent 8890) and a battery tester, etc.

[0056] Embodiment 1:

[0057] A method for preparing a positive electrode of a lithium-carbon dioxide battery with a charging potential lower than 3.0V, comprising:

[0058] a) 1.0 g of polyacrylonitrile and 0.5 g of polyvinyl pyrrolidone were added to 10 g of N,N-dimethylformamide and stirred magnetically at 60° C. for 12 h to obtain an electrospinning precursor solution.

[0059] b) A certain amount of the electrospinning precursor liquid in a) was taken into a 10 mL syringe, and a polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane was obtained by electrospinning. The electrospinning process parameters were: temperature 30°C, average humidity 35%, receiving distance 15 cm, positive high voltage 14 KV, negative high voltage -2.5 KV, syringe translation speed 2 mm / s, and drum speed 100 r / min.

[0060] c) drying the polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane in b) in a vacuum oven at 60° C. for 12 h.

[0061] d) The polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane dried in c) was subjected to cyclization and oxidation treatment in a muffle furnace at 260°C.

[0062] e) carbonizing the oxidized polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane in d) in a protective atmosphere to obtain nitrogen-rich three-dimensional self-supporting carbon fibers (nitrogen-doped carbon nanofiber membrane).

[0063] f) The nitrogen-doped carbon nanofiber membrane obtained in e) is placed in a culture dish, a certain amount of 0.25 M chloroplatinic acid and 1.25 M cobalt chloride aqueous solution is added, and the membrane is immersed in a stirring state for 30 minutes, and then the nitrogen-doped carbon nanofiber membrane is placed in liquid nitrogen for rapid freezing, and then freeze-dried.

[0064] g) The freeze-dried nitrogen-doped carbon nanofiber membrane in f) was heat treated at 450°C for 2 h in a mixture of argon and hydrogen at a heating rate of 5°C / min to obtain a CoPt@NCNF self-supporting catalytic positive electrode.

[0065] Comparative Example 1

[0066] The method is basically the same as Example 1, except that the aqueous solution of 0.25M chloroplatinic acid and 1.25M cobalt chloride in f) is replaced with an aqueous solution of 0.25M chloroplatinic acid to obtain a Pt@NCNF positive electrode.

[0067] Comparative Example 2

[0068] The method is basically the same as Example 1, except that the 0.25M chloroplatinic acid and 1.25M cobalt chloride aqueous solutions in f) are replaced with 1.25M cobalt chloride aqueous solution to obtain a Co@NCNF positive electrode.

[0069] The physical and chemical properties of the CoPt@NCNF self-supporting catalytic cathode were characterized:

[0070] Figure 1 This is a scanning electron micrograph of the CoPt@NCNF self-supporting catalytic cathode. It can be seen that there is no obvious agglomeration of the CoPt alloy nanoparticles. Figure 2 The X-ray diffraction diagram of the positive electrode of CoPt@NCNF and Pt@NCNF shows that compared with Pt nanoparticles, after CoPt alloying, each crystal plane moves to a high angle, proving that the interplanar spacing is compressed. This lattice strain can adjust the d-band center of Pt to move downward, thereby promoting the desorption of reaction intermediates on the Pt surface. Figure 3 This is a high-angle annular dark-field scanning transmission electron micrograph of Pt nanoparticles in the Pt@NCNF catalytic cathode. It can be seen from the figure that the interplanar spacings of Pt (200) and Pt (220) are 0.199 nm and 0.139 nm, respectively. Figure 4 This is a high-angle annular dark-field scanning transmission electron micrograph of CoPt nanoparticles in the CoPt@NCNF catalytic cathode. It can be seen from the figure that the interplanar spacings of Pt(200) and Pt(220) are 0.192nm and 0.132nm, respectively, which is consistent with Figure 3 Compared with the Pt nanoparticles in the sample, both the Pt(200) and Pt(220) crystal planes show obvious compression.

[0071] Characterization of the electrochemical properties of the CoPt@NCNF catalytic cathode:

[0072] Figure 5 The results show that the Li-CO2 battery based on three catalytic cathodes, CoPt@NCNF, Pt@NCNF and Co@NCNF, has a good performance at 20 μA cm -2 Current density, 100μAh cm -2 Comparison of discharge-charge performance at cut-off capacity. It can be seen from the figure that the discharge potential of the CoPt@NCNF cathode is significantly reduced, even though the cut-off potential is still below 3.0V, and the CoPt@NCNF cathode also exhibits a lower overpotential.

[0073] Characterization of the charge and discharge mechanism of the CoPt@NCNF catalytic cathode:

[0074] Figure 6 For lithium-carbon dioxide batteries at 50 μA cm -2 Current density, 500μAh cm -2Scanning electron microscope images of the CoPt@NCNF catalytic cathode after discharge and charge at the cut-off capacity. It can be seen from the figure that after discharge, the electrode surface is covered with a uniform layer of nanosheets, and after charging, the electrode surface returns to its original state, proving that the CoPt@NCNF catalytic cathode can effectively catalyze the decomposition of discharge products. Figure 7 For lithium-carbon dioxide batteries at 50 μA cm -2 Current density, 500μAh cm -2 X-ray diffraction patterns of CoPt@NCNF catalytic cathode before, after and after discharge at cut-off capacity. As can be seen from the figure, the generation and decomposition of lithium carbonate accompanies the charge and discharge process, proving that Figure 6 The solid discharge product is lithium carbonate. Figure 8 The results show that the cathode lithium-carbon dioxide battery based on CoPt@NCNF, Pt@NCNF and Co@NCNF catalyzes the -2 Current density, 500μAh cm -2 Gas mass spectrometer of gas phase products after discharge at cut-off capacity. As can be seen from the figure, compared with Pt@NCNF and Co@NCNF cathodes, CoPt@NCNF cathode contains a large amount of carbon monoxide in the gas phase after discharge, proving that the present invention successfully realizes a lithium-carbon dioxide battery with carbon monoxide as the main discharge product.

[0075] Embodiment 2-6:

[0076] A method for preparing a positive electrode of a lithium-carbon dioxide battery with a charging potential lower than 3.0V

[0077] In this example, CoPt@NCNF cathode catalyst for lithium-carbon dioxide battery was prepared respectively. The steps were basically the same as steps ag in Example 1, except that the types of raw materials, amounts and process parameters were different. See Table 1 for details.

[0078] Table 1 List of raw material types, dosages and process parameters for Examples 2-6

[0079]

[0080] Embodiment 7-10:

[0081] Development of a lithium-carbon dioxide battery with a charging potential lower than 3.0V

[0082] The lithium-carbon dioxide battery cathode catalyst prepared by the preparation method and process parameters in Example 1 was used to screen the battery electrolyte and the diaphragm. The battery structure is as follows: Fig. 9 shown.

[0083] The assembly and testing of lithium-carbon dioxide batteries were carried out in the following order: a CR2032 positive electrode shell with vent holes, CoPt@NCNF, Pt@NCNF or Co@NCNF positive electrode and a separator were placed in sequence, and then 80μL of electrolyte was dripped on the separator, and lithium metal negative electrode, current collector, shrapnel and CR2032 negative electrode shell were placed. After packaging, the above batteries were transferred to a self-made test device, CO2 gas was introduced for 50 minutes, and then left to stand for 12 hours before the electrochemical performance test was carried out.

[0084] The specific combination method for screening lithium-carbon dioxide battery electrolyte and diaphragm is shown in Table 2.

[0085] Table 2 Summary of electrolyte and diaphragm matching

[0086]

[0087] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A CoPt@NCNF electrode, characterized in that: The invention comprises a nitrogen-doped carbon nanofiber membrane and a cobalt-platinum alloy loaded on the nitrogen-doped carbon nanofiber membrane.

2. The CoPt@NCNF electrode according to claim 1, characterized in that The molar ratio of cobalt to platinum in the cobalt-platinum alloy is (0.1-0.3):(0.5-3).

3. The method for preparing the CoPt@NCNF electrode according to claim 1 or 2, characterized in that: include: S1, adding the nitrogen-doped carbon nanofiber membrane into an aqueous solution of chloroplatinic acid and cobalt chloride, immersing the membrane under stirring, and then freeze-drying the nitrogen-doped carbon nanofiber membrane; S2, heat treating the freeze-dried nitrogen-doped carbon nanofiber membrane in a mixture of inert gas and hydrogen at 300-700° C. to obtain the CoPt@NCNF electrode.

4. The method for preparing the CoPt@NCNF electrode according to claim 3, characterized in that: In S1, the method for preparing the nitrogen-doped carbon nanofiber membrane comprises: (1) adding polyacrylonitrile and polyvinyl pyrrolidone into N,N-dimethylformamide and stirring to obtain an electrospinning precursor solution; (2) The electrospinning precursor solution is electrospinned to obtain a polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane; the mass ratio of polyacrylonitrile, polyvinyl pyrrolidone and N,N-dimethylformamide is (1.0-1.4):0.5:(8-12); (3) drying the polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane and pre-oxidizing it at 200-280° C.; (4) The pre-oxidized polyacrylonitrile-polyvinyl pyrrolidone nanofiber membrane is carbonized in a protective atmosphere to obtain a nitrogen-doped carbon nanofiber membrane.

5. The method for preparing the CoPt@NCNF electrode according to claim 3, characterized in that: In S1, in the aqueous solution, the concentration of chloroplatinic acid is 0.1-0.3M, and the concentration of cobalt chloride is 0.5-3M.

6. The method for preparing the CoPt@NCNF electrode according to claim 3, characterized in that: In S1, the immersion time is 10-60 min.

7. The method for preparing the CoPt@NCNF electrode according to claim 3, characterized in that: In S2, the heat treatment time is 1-4h.

8. A lithium-carbon dioxide battery, characterized in that: It comprises a positive electrode, a separator and a negative electrode; the separator is located between the positive electrode and the negative electrode, and the positive electrode is the CoPt@NCNF electrode according to claim 1 or 2.

9. The lithium-carbon dioxide battery according to claim 8, characterized in that: The separator is glass fiber, polyimide, polyvinylidene fluoride-hexafluoropropylene or cellulose.

10. The lithium-carbon dioxide battery according to claim 8, characterized in that: The diaphragm is filled with an electrolyte, which is a dimethyl sulfoxide solution of lithium perchlorate, a dimethyl sulfoxide solution of lithium bis(trifluoromethylsulfonyl imide), a triethylene glycol dimethyl ether solution of lithium bis(trifluoromethylsulfonyl imide), or a tetraethylene glycol dimethyl ether solution of lithium bis(trifluoromethylsulfonyl imide).