Graft-modified sulfonated polybenzimidazole composite membrane for vanadium battery and preparation method of graft-modified sulfonated polybenzimidazole composite membrane

By introducing hydrophobic and hydrophilic side chains into the sulfonated polybenzimidazole membrane, the problem of low proton conductivity in vanadium redox flow batteries was solved, and the overall performance of vanadium batteries was improved.

CN118899489AInactive Publication Date: 2024-11-05HANGZHOU DEHAI AIKE ENERGY TECH CO LTD

Patent Information

Application Number
CN202411393058.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118899489A_ABST
    Figure CN118899489A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ion conducting membranes of all-vanadium redox flow batteries, and discloses a graft-modified sulfonated polybenzimidazole composite membrane for a vanadium battery and a preparation method thereof, and the composite membrane is prepared by grafting and modifying sulfonated polybenzimidazole, connecting hydrophobic flexible branched chains and hydrophilic branched chains and then forming the membrane. The preparation method further comprises the following steps: S1, preparing a sulfonated polybenzimidazole solution; s2, preparing a hydrophobic branch chain grafted modified sulfonated polybenzimidazole solution; s3, preparing a hydrophilic and hydrophobic branch chain grafted modified sulfonated polybenzimidazole solution; and S4, preparing the grafted modified sulfonated polybenzimidazole composite membrane. A chain segment of the grafted modified sulfonated polybenzimidazole polymer has hydrophilic and hydrophobic branched chains, and the comprehensive performance of the composite membrane can be regulated and controlled by regulating and controlling the proportion of the hydrophilic and hydrophobic branched chains, so that the composite membrane has high proton conduction density while having the characteristic of high vanadium resistance, and the energy efficiency of a vanadium battery is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange membranes for all-vanadium liquid flow batteries, and in particular to a grafted modified sulfonated polybenzimidazole composite membrane for vanadium batteries and a preparation method thereof. Background Art

[0002] In all-vanadium liquid flow batteries (VRFBs), cation exchange membranes (CEMs) have excellent proton conductivity, such as DuPont's Nafion series membranes, sulfonated polyimides, sulfonated polysulfones, and sulfonated polyetheretherketones. However, the severe penetration of vanadium ions has hindered the future development of CEMs in VRFBs. Polybenzimidazole (PBI) is a polymer with a heterocyclic ring that shows excellent chemical stability and mechanical properties in batteries. The positively charged alkaline heterocyclic imidazole groups in PBI can improve the selectivity of vanadium ions. In addition, PBI itself is relatively rigid and the membrane itself has narrow nanochannels, which greatly reduces the diffusion of vanadium ions and reduces the vanadium permeability.

[0003] Due to its excellent vanadium resistance and antioxidant properties, polybenzimidazole has great development and application prospects in vanadium flow batteries, but sulfonated polybenzimidazole membranes still have the problem of low proton conductivity. Summary of the invention

[0004] The purpose of the present invention is to provide a grafted modified sulfonated polybenzimidazole composite membrane for vanadium batteries and a preparation method thereof to solve the above problems.

[0005] The technical solution adopted by the present invention is as follows: A method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3-6 parts by mass of sulfonated polybenzimidazole to 100-150 parts by mass of a solvent, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution; Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1-0.3 parts by mass of chloroalkane to the sulfonated polybenzimidazole solution, then adding 0.1-0.3 parts by mass of a catalyst to the solution, and reacting in an oil bath at 70-90° C. for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution; Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1-0.3 parts by mass of monomer and 0.02-0.05 parts by mass of initiator to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 60-80° C. for reaction for 2-4 hours, and then adjusting the temperature to 40-60° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution; Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pouring the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, coating it with a scraper, and raising the temperature to 70-90° C. until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane.

[0006] Preferably, the solvent in step S1 is any one of dimethyl sulfoxide, N,N-dimethylacetamide and N,N-dimethylformamide.

[0007] Preferably, the chloroalkane in step S2 is any one of butyl chloride, hexyl chloride, octane chloride, isobutyl chloride, n-pentane chloride, dodecane chloride and tetradecane chloride.

[0008] Preferably, the catalyst in step S2 is any one of 4-dimethylaminopyridine, ammonium formate and sodium borohydride.

[0009] Preferably, the monomer in step S3 is any one of acrylamide, methacrylamide, acrylic acid, and 2-acrylamide-2-methylpropanesulfonic acid.

[0010] Preferably, the initiator in step S3 is any one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, and tert-butyl peroxide 2-ethyl acetate.

[0011] Preferably, the stirring and mixing speed in step S3 is 300-600 rpm.

[0012] Preferably, the thickness of the grafted modified sulfonated polybenzimidazole composite membrane in step S4 is 40-60 μm.

[0013] The graft modified sulfonated polybenzimidazole composite membrane for vanadium battery of the present invention is prepared by adopting the preparation method of the graft modified sulfonated polybenzimidazole composite membrane for vanadium battery.

[0014] The beneficial effects of the present invention are: 1. The present invention introduces hydrophobic flexible side chains into the sulfonated polybenzimidazole polymer chain segments, which can reduce the shuttling of vanadium ions through the steric hindrance effect and improve the coulombic efficiency of the vanadium battery.

[0015] 2. The sulfonated polybenzimidazole polymer chain segments of the present invention introduce hydrophilic side chains with ionic properties, which can increase the proton transfer density, maintain its high proton conductivity, reduce the internal resistance of the vanadium battery, and improve the voltage efficiency of the vanadium battery.

[0016] 3. The grafted modified sulfonated polybenzimidazole composite membrane of the present invention is an asymmetric membrane, which has both hydrophilic and hydrophobic side chains on the sulfonated polybenzimidazole polymer chain segment. The comprehensive performance of the composite membrane can be regulated by adjusting the ratio of the hydrophilic and hydrophobic side chains, so that the composite membrane has high vanadium resistance and high proton conduction density, thereby improving the energy efficiency of the vanadium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The infrared spectra of sulfonated benzimidazole, polyacrylamide and branch-modified sulfonated polybenzimidazole in Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0018] The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The present invention provides a method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery, comprising the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 3-6 parts by mass of sulfonated polybenzimidazole to 100-150 parts by mass of solvent, stirring at 80°C until completely dissolved, to obtain a sulfonated polybenzimidazole solution. The solvent is selected from any one of dimethyl sulfoxide, N,N-dimethylacetamide, and N,N-dimethylformamide; Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1-0.3 parts by mass of chloroalkane to the sulfonated polybenzimidazole solution, then adding 0.02-0.05 parts by mass of a catalyst to the solution, and reacting in an oil bath at 70-90°C for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution. The chloroalkane is selected from any one of butyl chloride, hexyl chloride, octane chloride, isobutyl chloride, n-pentane chloride, dodecane chloride, and tetradecane chloride; the catalyst is selected from any one of 4-dimethylaminopyridine, ammonium formate, and sodium borohydride; Step S3, prepare hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: add 0.1-0.3 parts by mass of monomer and 0.02-0.05 parts by mass of initiator to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution and stir and mix evenly, the stirring and mixing speed is 300-600rpm, heat to 60-80℃ for reaction for 2-4h, then adjust the temperature to 40℃-60℃ for 2 hours to obtain hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution. Among them, the monomer is selected from any one of acrylamide, methacrylamide, acrylic acid, and 2-acrylamide-2-methylpropanesulfonic acid; the initiator is selected from any one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, and tert-butyl peroxide 2-ethyl acid; Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pouring the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, coating it with a scraper, raising the temperature to 70-90°C until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 40-60 μm.

[0020] Embodiment 1:

[0021] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 4 parts by mass of sulfonated polybenzimidazole into 120 parts by mass of dimethyl sulfoxide as a solvent, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0022] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.2 parts by mass of chlorobutane to the sulfonated polybenzimidazole solution, and then adding 0.03 parts by mass of a catalyst 4-dimethylaminopyridine to the solution, and reacting in an 80° C. oil bath for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0023] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.2 parts by mass of monomer acrylamide and 0.03 parts by mass of initiator azobisisobutyronitrile to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 400 rpm, heating to 80° C. for reaction for 2 hours, and then adjusting the temperature to 60° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0024] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pour the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 80°C until the solvent is completely dried and evaporated to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 50 μm.

[0025] like Figure 1 As shown in the infrared spectrum of sulfonated polybenzimidazole, the -1 The out-of-plane deformation of the benzene ring in sulfonated polybenzyl imidazole can be observed in the range of 1057 cm -1 The stretching vibration of the S=O double bond in the sulfonic acid group was observed at 1614 cm -1 The stretching vibration of C=C and C=N is observed at the peak. In the infrared spectrum of polyacrylamide, it can be seen that the stretching vibration of C=C and C=N is at 1671 cm -1 A strong absorption peak of C=O stretching vibration of amide was observed at 100 nm. At the same time, this strong absorption peak can also be observed in the grafted modified sulfonated polybenzimidazole, which indicates that polyacrylamide has been successfully grafted onto sulfonated polybenzimidazole.

[0026] Embodiment 2:

[0027] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 3 parts by mass of sulfonated polybenzimidazole to 100 parts by mass of solvent N,N-dimethylacetamide, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0028] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1 parts by mass of hexyl chloride to the sulfonated polybenzimidazole solution, and then adding 0.02 parts by mass of a catalyst 4-dimethylaminopyridine to the solution, and reacting in an oil bath at 70° C. for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0029] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.2 parts by mass of monomer methacrylamide and 0.03 parts by mass of initiator azobisisoheptanenitrile to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 300 rpm, heating to 60° C. for reaction for 4 hours, and then adjusting the temperature to 40° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0030] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pouring the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, coating it with a scraper, raising the temperature to 70°C until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 40 μm.

[0031] Embodiment 3:

[0032] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 6 parts by mass of sulfonated polybenzimidazole to 150 parts by mass of solvent N,N-dimethylformamide, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0033] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.3 parts by mass of octyl chloride to the sulfonated polybenzimidazole solution, and then adding 0.04 parts by mass of catalyst ammonium formate to the solution, and reacting in a 90° C. oil bath for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0034] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1 parts by mass of monomer acrylic acid and 0.05 parts by mass of initiator benzoyl peroxide to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 500 rpm, heating to 70° C. for reaction for 3 hours, and then adjusting the temperature to 50° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0035] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pour the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a scraper, and raise the temperature to 90° C. until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 60 μm.

[0036] Embodiment 4:

[0037] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 5 parts by mass of sulfonated polybenzimidazole into 140 parts by mass of dimethyl sulfoxide as a solvent, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0038] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.2 parts by mass of isobutylene chloride to the sulfonated polybenzimidazole solution, and then adding 0.03 parts by mass of a catalyst sodium ammonium borohydride to the solution, and reacting in an oil bath at 85° C. for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0039] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.3 parts by mass of monomer 2-acrylamide-2-methylpropanesulfonic acid and 0.04 parts by mass of initiator 2-ethyl peroxide tert-butyl ester to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 600 rpm, heating to 75° C. for reaction for 3 hours, and then adjusting the temperature to 55° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0040] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pour the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a scraper, and raise the temperature to 80°C until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 55 μm.

[0041] Embodiment 5:

[0042] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 3 parts by mass of sulfonated polybenzimidazole into 100 parts by mass of dimethyl sulfoxide as a solvent, stirring at 80° C. until the polybenzimidazole is completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0043] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.3 parts by mass of n-pentyl chloride to the sulfonated polybenzimidazole solution, and then adding 0.03 parts by mass of azobisisobutyronitrile as a catalyst to the solution, and reacting in an oil bath at 75° C. for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0044] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1 parts by mass of monomer acrylamide and 0.03 parts by mass of initiator azobisisobutyronitrile to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 300 rpm, heating to 65° C. for reaction for 3 hours, and then adjusting the temperature to 45° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0045] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pour the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a scraper, and raise the temperature to 75°C until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 45 μm.

[0046] Embodiment 6:

[0047] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 4 parts by mass of sulfonated polybenzimidazole to 120 parts by mass of solvent N,N-dimethylacetamide, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0048] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.2 parts by mass of chlorododecane to the sulfonated polybenzimidazole solution, and then adding 0.03 parts by mass of a catalyst 4-dimethylaminopyridine to the solution, and reacting in an 80° C. oil bath for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0049] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.2 parts by mass of monomer methacrylamide and 0.03 parts by mass of initiator benzoyl peroxide to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 400 rpm, heating to 80° C. for reaction for 2 hours, and then adjusting the temperature to 60° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0050] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pouring the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, coating it with a scraper, and raising the temperature to 85° C. until the solvent is completely dried and volatilized to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 55 μm.

[0051] Embodiment 7:

[0052] A method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, preparation of sulfonated polybenzimidazole solution: adding 5 parts by mass of sulfonated polybenzimidazole to 140 parts by mass of solvent N,N-dimethylacetamide, stirring at 80° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0053] Step S2, preparing a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1 parts by mass of tetradecane chloride to the sulfonated polybenzimidazole solution, and then adding 0.05 parts by mass of a catalyst 4-dimethylaminopyridine to the solution, and reacting in an oil bath at 85° C. for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0054] Step S3, preparing a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.3 parts by mass of monomer acrylamide and 0.04 parts by mass of initiator azobisisobutyronitrile to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing at 400 rpm, heating to 70° C. for reaction for 2 hours, and then adjusting the temperature to 50° C. for 2 hours to obtain a hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution.

[0055] Step S4, preparing a grafted modified sulfonated polybenzimidazole composite membrane: pour the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 80°C until the solvent is completely dried and evaporated to obtain a grafted modified sulfonated polybenzimidazole composite membrane with a thickness of 50 μm.

[0056] Comparative Example 1 Preparation of sulfonated polybenzimidazole blank film: Pour the sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a doctor blade, and raise the temperature to 80°C until the solvent is completely dried and evaporated to obtain a sulfonated polybenzimidazole blank film with a film thickness of 50 μm.

[0057] Comparative Example 2 The same as Example 1, excluding step S2.

[0058] Comparative Example 3 The same as Example 1, excluding step S3.

[0059] The embodiment and comparative example membranes were assembled into a stack for testing, and the coulombic efficiency, voltage efficiency and energy efficiency were tested and recorded under the same test conditions. The test results are shown in the following table: Table 1: Battery performance test table of battery stacks assembled using the membranes of the embodiments and the comparative examples

[0060] It can be seen that Example 1 has a higher coulombic efficiency than Comparative Example 2, indicating that the present invention introduces hydrophobic flexible side chains into the sulfonated polybenzimidazole polymer chain segment, which can reduce the shuttling of vanadium ions through the steric hindrance effect, thereby improving the coulombic efficiency of the vanadium battery. Example 1 has a higher voltage efficiency than Comparative Example 3, indicating that the present invention introduces hydrophilic side chains with ionic characteristics into the sulfonated polybenzimidazole polymer chain segment, which can improve the proton transmission density, maintain its high proton conductivity, reduce the internal resistance of the vanadium battery, and improve the voltage efficiency of the vanadium battery. The embodiment has higher coulombic efficiency, voltage efficiency and energy efficiency than Comparative Example 1, because the grafted modified sulfonated polybenzimidazole composite membrane of the present invention is an asymmetric membrane, which has hydrophilic and hydrophobic side chains on the sulfonated polybenzimidazole polymer chain segment at the same time, and the comprehensive performance of the composite membrane can be regulated by adjusting the ratio of hydrophilic and hydrophobic side chains, so that the composite membrane has high proton conduction density while having high vanadium resistance, thereby improving the energy efficiency of the vanadium battery.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium batteries, characterized in that: The following steps are involved: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3-6 parts by mass of sulfonated polybenzimidazole to 100-150 parts by mass of a solvent, stirring at 80° C. until the sulfonated polybenzimidazole is completely dissolved, to obtain a sulfonated polybenzimidazole solution; Step S2, preparation of a hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1-0.3 parts by mass of chloroalkane to the sulfonated polybenzimidazole solution, then adding 0.1-0.3 parts by mass of a catalyst to the solution, and reacting in an oil bath at 70-90° C. for 24 hours to obtain a hydrophobic branched grafted modified sulfonated polybenzimidazole solution; Step S3, preparation of hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution: adding 0.1-0.3 parts by mass of monomer and 0.02-0.05 parts by mass of initiator to the hydrophobic branched grafted modified sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 60-80° C. for reaction for 2-4 hours, and then adjusting the temperature to 40-60° C. for 2 hours to obtain the hydrophilic and hydrophobic branched grafted modified sulfonated polybenzimidazole solution; Step S4, preparation of graft modified sulfonated polybenzimidazole composite membrane: pour the hydrophilic and hydrophobic branched graft modified sulfonated polybenzimidazole solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 70-90° C. until the solvent is completely dried and volatilized to obtain a graft modified sulfonated polybenzimidazole composite membrane.

2. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium battery according to claim 1, characterized in that: In step S1, the solvent is any one of dimethyl sulfoxide, N,N-dimethylacetamide, and N,N-dimethylformamide.

3. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium battery according to claim 1, characterized in that: In step S2, the chloroalkane is any one of butyl chloride, hexyl chloride, octane chloride, isobutyl chloride, n-pentane chloride, dodecane chloride and tetradecane chloride.

4. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium battery according to claim 1, characterized in that: In step S2, the catalyst is any one of 4-dimethylaminopyridine, ammonium formate, and sodium borohydride.

5. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium battery according to claim 1, characterized in that: In step S3, the monomer is any one of acrylamide, methacrylamide, acrylic acid, and 2-acrylamide-2-methylpropanesulfonic acid.

6. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: In step S3, the initiator is any one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, and tert-butyl peroxide 2-ethyl acetate.

7. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: The stirring and mixing speed in step S3 is 300-600 rpm.

8. The method for preparing a graft-modified sulfonated polybenzimidazole composite membrane for vanadium battery according to claim 1, characterized in that: The thickness of the grafted modified sulfonated polybenzimidazole composite membrane in step S4 is 40-60 μm.

9. A grafted modified sulfonated polybenzimidazole composite membrane for vanadium battery, characterized in that: The composite membrane is prepared by the method for preparing a grafted modified sulfonated polybenzimidazole composite membrane for vanadium batteries as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composition for the bottom layer of a resist, and method using same to manufacture a semiconductor integrated circuit device

    CN102687075A

  • Hydrophobic side chain-modified alkyl sulfonated polybenzimidazole amphoteric membrane and preparation method thereof

    CN108878936A

  • High proton transport exchange membrane for vanadium battery as well as preparation method and application of high proton transport exchange membrane

    CN115939477A

  • New tri:cyclic azepine derivatives inhibit cell-cell and cell-matrix interactions

    DE19612376A1

  • Solid electrolyte, manufacturing method of solid electrolyte, electrode for fuel cell, membrane and electrode assembly, and fuel cell

    JP2006236838A

Cited By

  • Preparation method and application of polybenzimidazole membrane regulated and controlled by grafting cross-linking strategy

    CN120535745A