Lithium ion battery disassembling and material recycling method
Through automated identification and intelligent disassembly technology, the problems of low lithium recovery and safety in lithium battery recycling are solved, and efficient direct recycling of waste lithium batteries and high-purity material regeneration are achieved, which improves production efficiency and resource recovery.
Patent Information
- Application Number
- CN202411015707.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-05
AI Technical Summary
During the recycling process of existing lithium batteries, there are problems such as low lithium recovery rate, high risk of liquid waste generated by wet crushing, high energy consumption and unsafe disassembly, especially in terms of precise separation of electrode materials and purification.
Using automated identification and intelligent disassembly technology, through visual measurement, cutting, molten salt heating and deep learning recognition, the lossless disassembly and efficient direct recycling of waste lithium batteries, including discharge treatment, cutting, washing, and molten salt recycling. and the freezing and curing and purification of electrolytes to ensure safe production and regeneration of high-purity materials.
Resource recycling and utilization of waste lithium batteries has been realized, lithium recycling rate and production efficiency have been improved, energy consumption and hazardous waste production have been reduced, and process safety and efficiency have been ensured.
Smart Images

Figure CN118899573A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fine disassembly and secondary recycling of waste lithium batteries, and in particular to a lithium ion battery disassembly and material recycling method. Background Art
[0002] Lithium batteries are becoming increasingly important in our lives. They are widely used in electronic products, electric vehicles and other fields because of their high specific capacity and good cycle performance. The demand for lithium batteries will grow explosively. It is estimated that by 2030, the global lithium-ion battery market demand in the electric vehicle field alone will reach 550 megawatt-hours. Generally, the life of lithium batteries is about 3-5 years, and more than 2 million tons of waste lithium-ion batteries are generated each year, but they and their electrolytes contain valuable materials such as cobalt, copper, aluminum, nickel, and lithium. Therefore, the regeneration of positive electrode materials and the recycling of electrolytes are one of the effective ways to solve the shortage of resources and environmental pollution in the battery industry, and help to establish an efficient circular economy.
[0003] The first step of conventional recycling is the pretreatment of used lithium batteries and the classification of battery components. Existing pretreatment uses mechanical processes such as crushing and shredding to expose valuable electrode materials for subsequent hydrometallurgy and pyrometallurgy, but it has disadvantages such as low lithium recovery rate, high generation of hazardous liquid waste by wet crushing, and high energy consumption. In contrast, efficient direct recycling processes can directly recover and reuse battery materials in the supply chain without destroying the chemical structure. In theory, everything in used lithium batteries can be recovered through the direct recycling process, including positive electrode materials, electrolytes, diaphragms, aluminum and graphite. However, one of the challenges of direct recycling of battery-grade materials is the precise separation and purification of electrode materials. Traditional crushing methods introduce a large amount of impurities such as copper and aluminum into the positive electrode materials, increasing the difficulty of downstream recycling. Traditional manual disassembly of used lithium batteries is impractical, and workers are exposed to toxic substances and there is a risk of battery explosion. At the same time, the disassembly of used lithium batteries varies due to manufacturers, process parameters, vehicle models, number of cycles, health status, etc., so automatic disassembly without human intervention is the first choice for direct recycling preprocessing. The key to disassembly under complex and changing conditions lies in the combination of non-destructive testing and identification, automation and intelligence. Summary of the invention
[0004] The present invention aims to solve the problems of separation of waste materials, recovery of high-purity positive electrode materials and green recovery and treatment of electrolyte in the process of lithium battery recovery, and further provides a lithium ion battery disassembly and material recovery method.
[0005] The present invention discloses a lithium ion battery disassembly and material recovery method which is specifically carried out in the following steps:
[0006] 1. Perform visual inspection on the collected waste lithium batteries, and discharge those that meet the standards to obtain discharged waste lithium batteries;
[0007] 2. Disassemble the used lithium batteries after discharge and cut them according to the actual size of the batteries; after cutting, take out the batteries and put them in a tray for washing to obtain the used positive electrode materials, and send the used positive electrode materials to the positive electrode material regeneration area. The electrolyte dropped during the cutting process is collected and transported to the electrolyte recovery area;
[0008] 3. Recycling the waste cathode material by heating in molten salt to obtain regenerated LiCoO2;
[0009] Fourth, the recovered electrolyte is frozen and solidified, and then liquid nitrogen is added to obtain a solidified lithium-rich electrolyte; the solidified lithium-rich electrolyte is chopped and ground, leached with acid and alkali solutions, purified with EDTA, and precipitated with calcium carbonate to obtain lithium carbonate, a raw material for the positive electrode of a lithium battery.
[0010] Beneficial effects of the present invention:
[0011] The present invention realizes the resource recycling of waste lithium batteries, including automatic identification of waste lithium battery recycling, secondary recycling of waste electrolyte and reusable regeneration of waste positive electrode materials.
[0012] Compared with the problems of low lithium recovery rate, large amount of liquid hazardous waste generated by wet crushing, high energy input and so on in hydrometallurgy and pyrometallurgy, the automatic identification disassembly and efficient direct recycling process of the present invention can directly recycle and reuse battery materials in the supply chain without destroying their chemical structure, thereby increasing the yield of high-value products.
[0013] The present invention uses the computer's curled neural network deep learning to identify and screen waste lithium batteries of different sizes, different companies, and different types, and disassembles them under a cutter equipped with a temperature controller and a temperature alarm to separate the positive electrode, negative electrode, and electrolyte of the battery core, thereby ensuring production safety and preventing the waste battery from catching fire and exploding. At the same time, the regeneration of the waste positive electrode adopts a two-stage heating method, and O2 and LiNO3 are introduced into the molten salt of different systems to regenerate the degraded LiCoO2, which can effectively remove all complex impurities without destroying the structure of the electrode material. The regenerated positive electrode material is repaired to the commercial level in structure, composition, and morphology, which can be comparable to commercial positive electrode materials, not only shortening the purification process, but also improving production efficiency and resource recovery rate. In addition, the present invention also provides a method for preparing lithium carbonate by electrolyte hydrometallurgy, which realizes the green recovery of waste lithium battery electrolyte through leaching, purification, and precipitation, which is conducive to large-scale industrial production and has good practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a SEM image of the waste positive electrode material in the embodiment;
[0015] Figure 2This is a SEM image of lithium carbonate, a raw material for the positive electrode of a lithium battery in the embodiment;
[0016] Figure 3 It is a physical picture of the waste lithium battery in the embodiment. DETAILED DESCRIPTION
[0017] The following embodiments are described with reference to the accompanying drawings.
[0018] Specific implementation method 1: In this implementation method, a lithium-ion battery disassembly and material recovery method is specifically carried out in the following steps:
[0019] 1. Perform visual inspection on the collected waste lithium batteries, and discharge those that meet the standards to obtain discharged waste lithium batteries;
[0020] 2. Disassemble the used lithium batteries after discharge and cut them according to the actual size of the batteries; after cutting, take out the batteries and put them in a tray for washing to obtain the used positive electrode materials, and send the used positive electrode materials to the positive electrode material regeneration area. The electrolyte dropped during the cutting process is collected and transported to the electrolyte recovery area;
[0021] 3. Recycling the waste cathode material by heating in molten salt to obtain regenerated LiCoO2;
[0022] Fourth, the recovered electrolyte is frozen and solidified, and then liquid nitrogen is added to obtain a solidified lithium-rich electrolyte; the solidified lithium-rich electrolyte is chopped and ground, leached with acid and alkali solutions, purified with EDTA, and precipitated with calcium carbonate to obtain lithium carbonate, a raw material for the positive electrode of a lithium battery.
[0023] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: if smoke, fire, leakage, distortion, serious damage or signs of human disassembly are found in the appearance inspection in step 1, it is considered to be non-compliant with the standards.
[0024] Specific implementation method three: The difference between this implementation method and specific implementation method one is that: the discharge treatment described in step one is to place the waste lithium battery into an electrolyte solution for discharge, and the treatment time is 24 hours; then the voltage of the waste lithium battery after discharge is detected to ensure that the residual voltage is not higher than 0.5V before the monomer is disassembled.
[0025] This embodiment adopts the technical specifications in the discharge technical specification DB34 / T 3077-2018 to perform voltage detection after discharge.
[0026] Specific implementation method 4: This implementation method is different from specific implementation method 3 in that the electrolyte solution is 0.8 mol / L NaCl, 0.8 mol / L ferrous sulfate solution or 1.2 mol / L manganese sulfate solution.
[0027] Specific implementation method five: This implementation method is different from specific implementation method one in that: the disassembly described in step two is to send the discharged used lithium batteries into a battery disassembly system composed of an automatic identification device for used lithium batteries and a battery cutting station; the battery cutting station is equipped with a thermal imager and a temperature alarm system; the automatic identification device for used lithium batteries is equipped with a high-precision camera and three optical degrees of freedom of focus, zoom, and aperture, and the size of the input image is adjusted to 100*100; the automatic identification device for used lithium batteries uses a convolutional neural network to perform deep learning on high-definition photos of used lithium batteries to deduce the actual size of the battery.
[0028] Specific implementation method six: This implementation method is different from specific implementation method five in that: the convolutional neural network described in step two uses the Bayesian optimization method to find the optimal configuration of the deep network; before formal processing, 150 photos of used lithium batteries of different sizes, manufacturers, and specifications are selected for training to establish a used lithium battery database, of which 100 images are used for verification to adjust hyperparameters, and the remaining 50 images are used for testing; the hyperparameters are set as follows: the filter size is 3, the initial learning rate is 0.0055, and the momentum is 0.85; after deep network classification, the recognition device marks each image according to the brand and size.
[0029] This embodiment can efficiently and automatically predict battery types on a large scale through the trained recognition device, and extract the best features of each individual waste battery for classification. Hyperparameters such as learning rate, epoch number, batch size, network depth, etc. determine the structure and settings of the convolutional neural network, and also determine the recognition rate of this recognition model. The convolutional neural network of the recognition device in the present invention mainly uses the Bayesian optimization (BO) method to find the best configuration of the deep network.
[0030] Specific implementation method seven: This implementation method is different from specific implementation method one in that: the cutting described in step two is carried out in the absence of oxygen, the waste lithium battery is fixed in a horizontal position by a mechanical clamp, the saw blade is placed vertically, and the mechanical clamp pushes the waste lithium battery toward the saw blade for cutting. The saw blade cutting speed is 2.73 to 4.17 m / s, the saw blade tooth density is 6 to 10 per centimeter, and the cutting and feeding speed of the mechanical clamp is 60 to 120 mm / min.
[0031] The battery cutting station equipped with a thermal imager and a temperature alarm system in this embodiment cuts according to different sizes after identification and classification; during the cutting process, a sudden increase in temperature will bring safety hazards. Therefore, it is necessary to monitor the temperature and prevent sudden temperature increases by adjusting the machine settings. Therefore, the thermal imager and temperature alarm system are implemented during the cutting process to monitor to prevent explosions and fires.
[0032] Specific implementation eight: This implementation differs from specific implementation one in that: the washing in step two is to pour 15% potassium sulfate brine into the tray, stir and wash for 20 minutes, and then let it stand for 1 hour.
[0033] Specific embodiment nine: This embodiment is different from specific embodiment one in that: in step three, the waste positive electrode material is recycled by heating in molten salt. The specific steps are as follows: the waste positive electrode material is put into a high-powered crusher for crushing and sieving through a 60-mesh screen; the diaphragm and the bulk metal current collector are separated and recovered to obtain the waste LiCoO2 containing impurities; the waste LiCoO2 containing impurities and the molten salt are put into an alumina crucible and heated to 300°C together with LiNO3 for reaction for 8 hours, and then heated to 500°C for reaction for 16 hours. During the reaction, air is continuously introduced at a rate of 840 ml / min. After the reaction is completed, it is washed with deionized water, filtered, and dried at 80°C for 12 hours to obtain regenerated LiCoO2; the speed of the high-powered crusher is controlled at 300-500r / min, and the duration is The time for pulverizing and screening is 30min. A closed environment is maintained during the crushing and screening process and a gas collection device is provided. The overflowed gas is dried with a desiccant P2O5, and finally the toxic gas is absorbed by an alkaline solution NaOH. The molar ratio of the mass of the molten salt to the waste LiCoO2 containing impurities is 1g:2mol; the molar ratio of the LiNO3 to the waste LiCoO2 containing impurities is 1:5; the formula of the molten salt is a LiOH-KCl binary salt system, a LiOH-KOH binary salt system or a Li2CO3-K2CO3 binary salt system; the mass ratio of LiOH to KCl in the LiOH-KCl molten salt system is 2:8; the mass ratio of LiOH to KOH in the LiOH-KOH molten salt system is 3:7, and the mass ratio of Li2CO3 to K2CO3 in the Li2CO3-K2CO3 molten salt system is 3:7.
[0034] The separator and the bulk metal current collector (Al foil and Cu foil) of this embodiment can be easily separated and recycled by sieve. Although the LiCoO2 powder obtained after sieving still contains a large amount of impurities, such as graphite, conductive agent, binder and trace amounts of Al and Cu, the molten salt regeneration method can remove different impurities and regenerate the LiCoO2 positive electrode material in one step without affecting its electrochemical performance.
[0035] Specific embodiment ten: This embodiment differs from specific embodiment one in that: in step four, the recovered electrolyte is frozen and solidified, and liquid nitrogen is added to obtain a solidified lithium-rich electrolyte; the solidified lithium-rich electrolyte is chopped and ground to a diameter of <0.1 mm, and the ground powder and a 6% sulfuric acid solution are placed together in a three-necked flask equipped with a magnetic stirrer and a condenser for leaching treatment; after selective leaching, sodium hydroxide is added to adjust the pH value of the leaching solution to 11 to obtain a leaching solution, and then EDTA is added at an addition amount of 3 g / L to purify the leaching solution to obtain a purified solution ; then add Na2CO3 solution to the purified solution at 95°C; then filter the precipitated lithium carbonate, wash with ultrapure water, and dry in air at 90°C for 10 hours to obtain lithium carbonate, a positive electrode raw material for a lithium battery; in the leaching treatment, every 100g of solidified lithium-rich electrolyte is dissolved in 200mL of a 6% sulfuric acid solution for leaching and maintaining a liquid-solid ratio of 2:1. The leaching reaction temperature is 80°C and the reaction time is 1h; the concentration of the Na2CO3 solution is 30%; the amount of the Na2CO3 solution added is: every 1L of purified solution corresponds to the mass of the solute in 500g of Na2CO3 solution.
[0036] After selective leaching in this embodiment, lithium is separated from other elements (calcium, magnesium, aluminum) and exists in the solution for further treatment, sodium hydroxide is added and the pH value of the leachate is adjusted and the pH value is measured using a pH meter (PHS-3C) to remove magnesium and aluminum ions and partially remove calcium ions, and then EDTA is added to further purify the resulting leached solution to remove calcium ions. Afterwards, a vacuum suction filter is used to remove solids containing impurities from the solution, thereby purifying the lithium sulfate in the solution. In order to obtain the highest recovery rate of lithium carbonate solids, the precipitated lithium carbonate is filtered, washed with ultrapure water to completely remove carbonates and sodium ions, and then dried to finally obtain lithium carbonate, a lithium battery positive electrode raw material with good performance.
[0037] The following examples are used to verify the beneficial effects of the present invention:
[0038] Embodiment: A lithium-ion battery disassembly and material recovery method is specifically carried out according to the following steps:
[0039] 1. Perform visual inspection on the collected automotive lithium iron phosphate waste batteries, and perform discharge treatment on those that meet the standards to obtain discharged waste lithium batteries; if smoke, fire, leakage, distortion, severe damage or traces of human disassembly are found in the appearance inspection, they are deemed not to meet the standards; the discharge treatment is to place the waste lithium batteries in a 1.2 mol / L manganese sulfate solution for discharge for 24 hours; then perform voltage detection on the discharged waste lithium batteries to ensure that the residual voltage is not higher than 0.5V before the monomer is disassembled;
[0040] 2. Send the discharged waste lithium batteries into the battery disassembly system for disassembly; send the discharged waste lithium batteries into the battery disassembly system composed of a waste lithium battery automatic identification device and a battery cutting station; the battery cutting station is equipped with a thermal imager and a temperature alarm system; the waste lithium battery automatic identification device is equipped with a high-precision camera and three optical degrees of freedom of focus, zoom and aperture, and the size of the input image is adjusted to 100*100; the waste lithium battery automatic identification device uses a convolutional neural network to perform deep learning on high-definition photos of waste lithium batteries to deduce the actual size of the battery; cut according to the actual size of the battery; after cutting, The battery cell is taken out and placed in a tray for washing to obtain waste positive electrode materials, and the waste positive electrode materials are sent to the positive electrode material regeneration area, and the electrolyte dropped during the cutting process is collected and transported to the electrolyte recovery area; the cutting is carried out in the absence of oxygen, the waste lithium battery is fixed in a horizontal position by a mechanical clamp, the saw blade is placed vertically, and the mechanical clamp pushes the waste lithium battery to the saw blade for cutting, the saw blade cutting speed is 3.00m / s, the saw blade has a sawtooth density of 6 to 10 per centimeter, and the cutting and sample delivery speed of the mechanical clamp is 100mm / min; the washing is to pour a potassium sulfate salt solution with a concentration of 15% into the tray, stir and wash for 20 minutes, and then stand for 1 hour;
[0041] 3. The waste positive electrode material is put into a high-powered pulverizer for crushing and sieving through a 60-mesh screen; the diaphragm and the bulk metal current collector are separated and recovered to obtain the waste LiCoO2 containing impurities; 10 mol of waste LiCoO2 containing impurities and 5 g of molten salt are put into an alumina crucible and heated to 300°C for reaction with 2 mol LiNO3 for 8 hours, and then heated to 500°C for reaction for 16 hours. During the reaction, air is continuously introduced at a rate of 840 ml / min. After the reaction is completed, it is washed with deionized water, filtered, and dried at 80°C for 12 hours to obtain regenerated LiCoO2; the speed of the high-powered pulverizer is controlled at 300-500 r / min, and the duration is 30 minutes. During the crushing and screening process, a closed environment is maintained and a gas collection device is provided. The overflowed gas is dried with a desiccant P2O5 Drying treatment, and finally absorbing the toxic gas by alkaline solution NaOH; the formula of the molten salt is LiOH-KCl binary salt system, LiOH-KOH binary salt system or Li2CO3-K2CO3 binary salt system; the mass ratio of LiOH to KCl in the LiOH-KCl molten salt system is 2:8; the mass ratio of LiOH to KOH in the LiOH-KOH molten salt system is 3:7, and the mass ratio of Li2CO3 to K2CO3 in the Li2CO3-K2CO3 molten salt system is 3:7;
[0042] 4. Freeze-solidify the recovered electrolyte, and then add liquid nitrogen to obtain a solidified lithium-rich electrolyte; chop and grind the solidified lithium-rich electrolyte to a diameter of <0.1 mm, and put the ground powder and a 6% sulfuric acid solution into a three-necked flask equipped with a magnetic stirrer and a condenser for leaching treatment; after selective leaching, add sodium hydroxide to adjust the pH value of the leaching solution to 11 to obtain a leaching solution, and then add EDTA at an addition amount of 3g / L to purify the leaching solution to obtain a purified solution; then add Na2CO3 solution to the purified solution at 95°C; the concentration of the Na2CO3 solution is 30%; the addition amount of the Na2CO3 solution is: 500g for every 1L of purified solution The mass of the solute in the Na2CO3 solution; the precipitated lithium carbonate is then filtered, washed with ultrapure water, and dried in air at 90°C for 10 hours to obtain lithium carbonate, a positive electrode raw material for a lithium battery; in the leaching treatment, every 100g of solidified lithium-rich electrolyte is dissolved in 200mL of a 6% sulfuric acid solution for leaching and maintaining a liquid-to-solid ratio of 2:1, the leaching reaction temperature is 80°C, and the reaction time is 1h.
[0043] In the NaOH and EDTA purification, lithium can be separated from other impurities by controlling the pH value of the leachate. The pH value of the leachate is 0.61, and the leachate is first neutralized to pH 11 with sodium hydroxide under optimal conditions (80°C, 20 minutes). The mass concentrations of the main elements before and after purification are listed in Table 2.
[0044] Table shows the removal efficiency and mass concentration of main elements before and after purification.
[0045]
[0046]
[0047] The main impurity elements in the leachate are magnesium, calcium and aluminum, and the removal rates after purification by NaOH are 99.2%, 75.7% and 99.8% respectively.
Claims
1. A method for disassembling a lithium-ion battery and recovering materials, characterized in that The disassembly and material recovery method of lithium-ion batteries is specifically carried out in the following steps:
1. Perform visual inspection on the collected waste lithium batteries, and discharge those that meet the standards to obtain discharged waste lithium batteries; 2. Disassemble the used lithium batteries after discharge and cut them according to the actual size of the batteries; after cutting, take out the batteries and put them in a tray for washing to obtain the used positive electrode materials, and send the used positive electrode materials to the positive electrode material regeneration area. The electrolyte dropped during the cutting process is collected and transported to the electrolyte recovery area; 3. Recycling the waste cathode material by heating in molten salt to obtain regenerated LiCoO2; Fourth, the recovered electrolyte is frozen and solidified, and then liquid nitrogen is added to obtain a solidified lithium-rich electrolyte; the solidified lithium-rich electrolyte is chopped and ground, leached with acid and alkali solutions, purified with EDTA, and precipitated with calcium carbonate to obtain lithium carbonate, a raw material for the positive electrode of a lithium battery.
2. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that If smoke, fire, leakage, distortion, severe damage or signs of human disassembly are found during the appearance inspection in step 1, it is deemed to be non-compliant with the standards.
3. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that The discharge treatment described in step 1 is to place the waste lithium battery into an electrolyte solution for discharge for 24 hours; then the voltage of the waste lithium battery after discharge is detected to ensure that the residual voltage is not higher than 0.5V before the monomer is disassembled.
4. A lithium-ion battery disassembly and material recovery method according to claim 3, characterized in that The electrolyte solution is 0.8 mol / L NaCl, 0.8 mol / L ferrous sulfate solution or 1.2 mol / L manganese sulfate solution.
5. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that The disassembly described in step 2 is to send the discharged waste lithium battery into a battery disassembly system composed of a waste lithium battery automatic identification device and a battery cutting station; the battery cutting station is equipped with a thermal imager and a temperature alarm system; the waste lithium battery automatic identification device is equipped with a high-precision camera and three optical degrees of freedom of focus, zoom, and aperture, and the size of the input image is adjusted to 100*100; the waste lithium battery automatic identification device uses a convolutional neural network to perform deep learning on high-definition photos of waste lithium batteries to deduce the actual size of the battery.
6. A lithium-ion battery disassembly and material recovery method according to claim 5, characterized in that The convolutional neural network described in step 2 uses the Bayesian optimization method to find the optimal configuration of the deep network; before formal processing, 150 photos of used lithium batteries of different sizes, manufacturers, and specifications are selected for training to establish a used lithium battery database, of which 100 images are used for verification to adjust hyperparameters, and the remaining 50 are used for testing; the hyperparameters are set as follows: the filter size is 3, the initial learning rate is 0.0055, and the momentum is 0.85; after deep network classification, the recognition device marks each image according to brand and size.
7. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that The cutting described in step 2 is carried out in an oxygen-free environment. The waste lithium battery is fixed in a horizontal position by a mechanical clamp, and the saw blade is placed vertically. The mechanical clamp pushes the waste lithium battery toward the saw blade for cutting. The saw blade cutting speed is 2.73 to 4.17 m / s, the saw blade tooth density is 6 to 10 per centimeter, and the cutting sample feeding speed of the mechanical clamp is 60 to 120 mm / min.
8. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that The washing in step 2 is to pour 15% potassium sulfate brine into the tray, stir and wash for 20 minutes and then let it stand for 1 hour.
9. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that In step three, the waste positive electrode material is recycled by heating in molten salt. The specific steps are as follows: the waste positive electrode material is put into a high-powered crusher for crushing and sieving through a 60-mesh screen; the diaphragm and the bulk metal current collector are separated and recovered to obtain the waste LiCoO2 containing impurities; the waste LiCoO2 containing impurities and the molten salt are put into an alumina crucible and heated to 300°C together with LiNO3 for reaction for 8 hours, and then heated to 500°C for reaction for 16 hours. During the reaction, air is continuously introduced at a rate of 840 ml / min. After the reaction is completed, it is washed with deionized water, filtered, and dried at 80°C for 12 hours to obtain regenerated LiCoO2; the speed of the high-powered crusher is controlled at 300-500 r / min, the duration is 30 minutes, and the crushing and sieving are carried out. During the process, a closed environment is maintained and a gas collection device is provided. The overflowed gas is dried with a desiccant P2O5, and finally the toxic gas is absorbed by an alkaline solution NaOH; the molar ratio of the mass of the molten salt to the waste LiCoO2 containing impurities is 1g:2mol; the molar ratio of the LiNO3 to the waste LiCoO2 containing impurities is 1:5; the formula of the molten salt is a LiOH-KCl binary salt system, a LiOH-KOH binary salt system or a Li2CO3-K2CO3 binary salt system; the mass ratio of LiOH to KCl in the LiOH-KCl molten salt system is 2:8; the mass ratio of LiOH to KOH in the LiOH-KOH molten salt system is 3:7, and the mass ratio of Li2CO3 to K2CO3 in the Li2CO3-K2CO3 molten salt system is 3:
7.
10. A lithium-ion battery disassembly and material recovery method according to claim 1, characterized in that Step 4: freeze-solidify the recovered electrolyte, and then add liquid nitrogen to obtain a solidified lithium-rich electrolyte; chop and grind the solidified lithium-rich electrolyte to a diameter of <0.1 mm, and put the ground powder and a 6% sulfuric acid solution into a three-necked flask equipped with a magnetic stirrer and a condenser for leaching treatment; after selective leaching, add sodium hydroxide to adjust the pH value of the leaching solution to 11 to obtain a leaching solution, and then add EDTA at an addition amount of 3 g / L to purify the leaching solution to obtain a purified solution; Then, Na2CO3 solution is added to the purified solution at 95°C; the precipitated lithium carbonate is then filtered, washed with ultrapure water, and dried in air at 90°C for 10 hours to obtain lithium carbonate, a positive electrode raw material for a lithium battery; in the leaching treatment, every 100g of solidified lithium-rich electrolyte is dissolved in 200mL of a 6% sulfuric acid solution for leaching and the liquid-solid ratio is maintained at 2:1, the leaching reaction temperature is 80°C, and the reaction time is 1h; the concentration of the Na2CO3 solution is 30%; the amount of the Na2CO3 solution added is: every 1L of purified solution corresponds to the mass of the solute in 500g of the Na2CO3 solution.