Preparation method of high-thermal-conductivity and high-electric-conductivity copper boron nitride composite material
By depositing multiple layers of hexagonal boron nitride on copper foil and adopting stacked hot pressing technology, the problems of poor wetting and interface bonding between hexagonal boron nitride and copper are solved, and the thermal conductivity of boron nitride copper composite material is improved and conductivity, and realize the controllability of the process and large-scale production.
Patent Information
- Application Number
- CN202411037684.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-05
AI Technical Summary
Poor wetting and poor interfacial bonding between hexagonal boron nitride and copper lead to a decrease in strength of the composite material, and it is easy to destroy the structure of hexagonal boron nitride during the preparation process, resulting in a far difference in performance from the theoretical value.
By depositing multiple layers of hexagonal boron nitride on both sides of the copper foil, a cladding structure is formed and a stacked hot pressing process is used to form a highly thermally conductive boron nitride copper composite material to ensure uniform dispersion and interface bonding of hexagonal boron nitride.
It improves the density and structure uniformity of composite materials, enhances thermal and electrical conductivity, and has good process controllability, which is suitable for large-scale production.
Smart Images

Figure CN118900539A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material manufacturing, and in particular to a method for preparing a high thermal and electrical conductivity boron nitride copper composite material. Background Art
[0002] Pure metals have long been considered to have the lowest conductivity at room temperature. Since the first official record of copper's conductivity about 100 years ago, a large number of studies on highly refined copper metal have only increased the conductivity by about 3%. The widely used International Annealed Copper Standard (IACS) records the conductivity of pure copper at room temperature as 5.8×10 7 S / m, among metals, only silver has a better electrical conductivity than copper (about 108% IACS), but the cost of silver is too high, so copper-based materials have been used as the main conductive material.
[0003] In order to improve the conductivity of copper-based materials, the method of preparing high-purity copper by increasing purity, reducing grain boundaries and reducing defects has gradually approached the physical limit, and the cost has increased significantly, and the technical requirements have become more and more stringent; and the addition of other alloy materials (such as tin, rare earth elements, etc.) also often has the phenomenon of decreased conductivity due to process instability or copper matrix lattice distortion, which has certain limitations; the use of metallic copper and new materials to prepare high thermal and electrical conductivity copper-based composite materials has attracted extensive research.
[0004] Hexagonal boron nitride (h-BN) is a hexagonal layered structure composed of nitrogen atoms and boron atoms. The atoms in the layer are connected by sp2 hybridization and the layers are bonded by van der Waals forces. Its structure is very similar to graphite. It is a loose, lubricated, moisture-absorbing, light-weight white powder, so it is called "white graphite". The theoretical thermal conductivity of a single layer of hexagonal boron nitride nanosheets (BNNS) can reach 1700-2000W / mK. In addition to excellent thermal conductivity, the elastic modulus of hexagonal boron nitride-based composite materials is increased to 70-80GPa, and the flexural strength reaches more than 200MPa. Due to its special two-dimensional structure and beneficial properties, hexagonal boron nitride still has good advantages in improving the mechanical properties of materials and maintaining the high electrical and thermal conductivity of copper, making it an excellent reinforcement material for copper-based composites. Hexagonal boron nitride-reinforced copper-based materials have been used in the automotive and aerospace industries.
[0005] However, the wettability between hexagonal boron nitride and copper is very poor, and the interface bonding between the two is poor, resulting in reduced material strength. In the preparation process of the composite material, the structure of hexagonal boron nitride is often destroyed, and the excellent performance of hexagonal boron nitride strongly depends on the complete structure. Therefore, the performance of the hexagonal boron nitride composite material obtained is often far from the theoretical value, and the mechanical and electrical properties of the metal matrix are reduced due to elastic incompatibility, so solving the problem of uniform dispersion of hexagonal boron nitride in the preparation process of hexagonal boron nitride copper composite material is a key issue. Summary of the invention
[0006] The present invention provides a method for preparing a high thermal and electrical conductivity boron nitride copper composite material, which comprises the following steps: S1: depositing multiple layers of hexagonal boron nitride on both sides of the copper foil to form a unit material hexagonal boron nitride coated copper foil; S2: placing the hexagonal boron nitride coated copper foil generated in step S1 in a hot pressing chamber, and the hexagonal boron nitride coated copper foil is not less than two pieces, and the at least two pieces of the hexagonal boron nitride coated copper foil are stacked and placed in a hot pressing mold, and the hexagonal boron nitride coated copper foil is stacked and hot-pressed into shape using a stacking hot pressing process to obtain a boron nitride copper composite material with high thermal conductivity and electrical conductivity.
[0007] The present invention is further configured as follows: the thickness of the hexagonal boron nitride coated copper foil in step S1 is 10-100 μm.
[0008] The present invention is further configured as follows: in step S1, the number of layers of hexagonal boron nitride deposited on the copper foil is 1-20 layers.
[0009] The present invention is further configured as follows: the hot pressing chamber is heated to 600-1100° C. for 20-100 minutes, then kept at a constant temperature for 20-100 minutes, and then cooled to room temperature after the insulation is completed for 20-100 minutes.
[0010] The present invention is further configured as follows: the hot pressing chamber is first pressurized to 20-200 MPa for 20-100 min, then maintained at a constant pressure for 20-100 min, and then depressurized to 0 MPa for 20-100 min.
[0011] The present invention is further configured as follows: the hot pressing chamber is maintained in vacuum or filled with argon gas for protection.
[0012] The beneficial effects of the present invention are as follows: the hexagonal boron nitride-coated copper foil is used as the base material, and the hexagonal boron nitride-copper composite material prepared by lamination hot pressing is more dense, uniform in structure, good in interface bonding, stable in performance, and has high thermal and electrical conductivity. At the same time, the process controllability of the method is good and it is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The process flow chart of the present invention is shown. DETAILED DESCRIPTION
[0014] Those skilled in the art can refer to the content of this article and appropriately improve the process parameters. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0015] The present invention provides a method for preparing a high thermal and electrical conductivity boron nitride copper composite material, comprising the following steps:
[0016] S1: depositing multiple layers of hexagonal boron nitride on both sides of the copper foil to form a unit material hexagonal boron nitride coated copper foil;
[0017] S2: placing the hexagonal boron nitride coated copper foil generated in step S1 in a hot pressing chamber, and the hexagonal boron nitride coated copper foil is not less than two pieces, and the at least two pieces of the hexagonal boron nitride coated copper foil are stacked and placed in a hot pressing mold, and the hexagonal boron nitride coated copper foil is stacked and hot-pressed into shape using a stacking hot pressing process to obtain a boron nitride copper composite material with high thermal conductivity and electrical conductivity.
[0018] The thickness of the hexagonal boron nitride coated copper foil deposited in step S1 is 10-100 μm.
[0019] The number of layers of hexagonal boron nitride deposited and coated on the copper foil in step S1 is 1-20 layers.
[0020] After the hexagonal boron nitride coated copper foil is stacked in step S2, the hot pressing chamber is heated to 600-1100°C for 20-100 minutes, and then kept at a constant temperature for 20-100 minutes. After the insulation is completed, it is cooled to room temperature for 20-100 minutes.
[0021] The pressure in the hot press chamber is increased to 20-200 MPa for 20-100 min, and then the constant pressure is maintained for 20-100 min. After the constant pressure is completed, the pressure is reduced to 0 MPa for 20-100 min.
[0022] It should be noted that the hot pressing chamber is maintained in vacuum or filled with argon gas for protection.
[0023] Example 1
[0024] The above method is used to prepare a high thermal and electrical conductivity boron nitride copper composite material, and the preparation process is as follows:
[0025] S1: depositing and coating a layer of hexagonal boron nitride on both sides of the copper foil to form a hexagonal boron nitride coated copper foil, and the thickness of the hexagonal boron nitride coated copper foil is 25 μm.
[0026] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0027] Before hot pressing, the material is heated to 800°C for 40 minutes and kept at a constant temperature for 40 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0028] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0029] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0030] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 261.5 W / (m·K) and the electrical conductivity was 106.2% IACS.
[0031] Example 2
[0032] S1: depositing and coating a layer of hexagonal boron nitride on both sides of the copper foil to form a hexagonal boron nitride coated copper foil, and the thickness of the hexagonal boron nitride coated copper foil is 50 μm.
[0033] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0034] Before hot pressing, the material is heated to 900°C for 40 minutes and kept at a constant temperature for 40 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0035] During the hot pressing process, the pressing intensity is 60MPa, the pressing time is 40min, the constant pressure time is 40min, and finally the pressure is reduced for 40min to reduce the pressure to 0MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0036] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0037] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 283.8.5 W / (m·K) and the electrical conductivity was 109.9% IACS.
[0038] Example 3
[0039] All conditions of step S1 of this embodiment are set the same as all conditions of step S1 in embodiment 2.
[0040] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0041] Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0042] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0043] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0044] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 256.3 W / (m·K) and the electrical conductivity was 111.9% IACS.
[0045] Example 4
[0046] All conditions of step S1 of this embodiment are set the same as all conditions of step S1 in embodiment 2.
[0047] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0048] Before hot pressing, the material is heated to 1000°C for 40 minutes and kept at a constant temperature for 80 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0049] During the hot pressing process, the pressing intensity is 75 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0050] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0051] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 301.4 W / (m·K) and the electrical conductivity was 112.5% IACS.
[0052] Example 5
[0053] All conditions of step S1 of this embodiment are set the same as all conditions of step S1 in embodiment 2.
[0054] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0055] Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0056] During the hot pressing process, the pressing intensity is 75 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0057] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0058] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 268.5 W / (m·K) and the electrical conductivity was 110.4% IACS.
[0059] Example 6
[0060] S1: 20 layers of hexagonal boron nitride are deposited and coated on both sides of the copper foil to form a hexagonal boron nitride coated copper foil, and the thickness of the hexagonal boron nitride coated copper foil is 50 μm.
[0061] All conditions of step S2 of this embodiment are set the same as all conditions of step S2 in embodiment 4.
[0062] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 343.2 W / (m·K) and the electrical conductivity was 106.5% IACS.
[0063] Example 7
[0064] S1: Ten layers of hexagonal boron nitride are deposited and coated on both sides of the copper foil to form a hexagonal boron nitride coated copper foil, and the thickness of the hexagonal boron nitride coated copper foil is 50 μm.
[0065] All conditions of step S2 of this embodiment are set the same as all conditions of step S2 in embodiment 4.
[0066] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 321.3 W / (m·K) and the electrical conductivity was 109.2% IACS.
[0067] Example 8
[0068] All conditions of step S1 of this embodiment are set the same as all conditions of step S1 in embodiment 2.
[0069] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0070] Before hot pressing, the material is heated to 600°C for 40 minutes and kept at a constant temperature for 80 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0071] During the hot pressing process, the pressing intensity is 75 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0072] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0073] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 224.7 W / (m·K) and the electrical conductivity was 103.2% IACS.
[0074] Example 9
[0075] All conditions of step S1 of this embodiment are set the same as all conditions of step S1 in embodiment 2.
[0076] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0077] Before hot pressing, the material is heated to 1000°C for 40 minutes and kept at a constant temperature for 80 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0078] During the hot pressing process, the pressing intensity is 20 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0079] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0080] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 267.4 W / (m·K) and the electrical conductivity was 104.4% IACS.
[0081] Example 10
[0082] All conditions of step S1 of this embodiment are set the same as all conditions of step S1 in embodiment 2.
[0083] S2: Take 16 pieces of hexagonal boron nitride coated copper foils generated in step S1 and put them into a hot pressing chamber, and then put the 16 pieces of hexagonal boron nitride into a hot pressing mold after stacking them for hot pressing.
[0084] Before hot pressing, the material is heated to 1000°C for 40 minutes and kept at a constant temperature for 80 minutes, during which time hot pressing is performed. After cooling for 40 minutes, the formed high thermal and electrical conductivity hexagonal boron nitride copper composite material is cooled to room temperature.
[0085] During the hot pressing process, the pressing intensity is 200 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 MPa, thereby obtaining a high thermal and electrical conductivity hexagonal boron nitride copper composite material.
[0086] In this embodiment, the hot pressing chamber maintains 1.0×10 -3 Vacuum degree of Pa.
[0087] The thermal conductivity and electrical conductivity of the high thermal and electrical conductivity hexagonal boron nitride copper composite material prepared in Example 1 were tested by transient method and Van der Pauw method, respectively, and the thermal conductivity was measured to be 310.6 W / (m·K) and the electrical conductivity was 110.1% IACS.
[0088] In summary, the present invention uses hexagonal boron nitride coated copper foil as the base material, and through lamination hot pressing, the hexagonal boron nitride copper composite material prepared is more dense, uniform in structure, good in interface bonding, stable in performance, and has high thermal and electrical conductivity. At the same time, the process controllability of the method is good and it is easy to mass produce.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be within the scope of protection of the present invention.
Claims
1. A method for preparing a high thermal and electrical conductivity boron nitride copper composite material, Features: The following steps are included: S1: depositing multiple layers of hexagonal boron nitride on both sides of the copper foil to form a unit material hexagonal boron nitride coated copper foil; S2: placing the hexagonal boron nitride coated copper foil generated in step S1 in a hot pressing chamber, and the hexagonal boron nitride coated copper foil is not less than two pieces, and the at least two pieces of the hexagonal boron nitride coated copper foil are stacked and placed in a hot pressing mold, and the hexagonal boron nitride coated copper foil is stacked and hot-pressed into shape using a stacking hot pressing process to obtain a high thermal and electrical conductivity boron nitride copper composite material.
2. The method for preparing the high thermal and electrical conductivity boron nitride copper composite material according to claim 1, Features: The hexagonal boron nitride coated copper foil in step S1 has a thickness of 10-100 μm.
3. The method for preparing the high thermal and electrical conductivity boron nitride copper composite material according to claim 1, Features: In step S1, the number of layers of hexagonal boron nitride deposited on the copper foil is 1-20 layers.
4. The method for preparing the high thermal and electrical conductivity boron nitride copper composite material according to claim 1, Features: The hot pressing chamber is heated to 600-1100° C. for 20-100 minutes, then kept at a constant temperature for 20-100 minutes, and then cooled to room temperature for 20-100 minutes.
5. The method for preparing the high thermal and electrical conductivity boron nitride copper composite material according to claim 1, Features: The hot pressing chamber is first pressurized to 20-200 MPa for 20-100 min, then kept at constant pressure for 20-100 min, and then depressurized to 0 MPa for 20-100 min after the constant pressure is completed.
6. The method for preparing the high thermal and electrical conductivity boron nitride copper composite material according to claim 1, Features: The hot pressing chamber is maintained in vacuum or filled with argon gas for protection.
Citation Information
Cited By
Patterned graphene copper composite material with high electric conductivity and heat conductivity and preparation method of patterned graphene copper composite material
CN119459047A
High-conductivity molybdenum disulfide copper composite material and preparation method thereof