High-elongation beryllium aluminum alloy and preparation method thereof
Through multiple vacuum smelting and rapid cooling processes, the defects in the solidification process of beryllium aluminum alloy are solved, the density and elongation of its internal tissue are improved, and the preparation of beryllium aluminum alloy is achieved.
Patent Information
- Application Number
- CN202411232858.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
The existing beryllium aluminum alloy is prone to defects such as shrinkage and shrinkage during solidification, resulting in inevitable defects inside the material, which cannot fully reflect the plasticity of aluminum-based composite materials. The existing technology mainly focuses on the increase in strength. It has little effect on plasticity improvement.
Multiple vacuum smelting methods are used to make beryllium and aluminum metal fully melt and mix evenly, and the beryllium aluminum alloy melt is quickly poured into a water-cooled mold for rapid cooling, which increases the internal tissue density of the alloy and thus increases the elongation.
Through this method, the internal structure uniformity and density of beryllium aluminum alloy are significantly improved, its elongation is enhanced, and defects such as shrinkage and shrinkage are reduced, thereby improving the plastic properties of the alloy.
Smart Images

Figure CN119082576A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of cast beryllium aluminum alloy, and in particular relates to a high-elongation beryllium aluminum alloy and a preparation method thereof. Background Art
[0002] Beryllium aluminum alloy is a light metal that combines the excellent properties of beryllium and aluminum. Beryllium aluminum alloy is superior to traditional structural metals in terms of low density, high specific strength and stiffness, high thermal conductivity and low thermal expansion coefficient, and has broad application prospects in industries such as aircraft, spacecraft and weapon equipment. Since aluminum and beryllium do not show obvious mutual solubility, they will not form intermetallic compounds together. Therefore, beryllium aluminum alloy is one of the most important multi-component materials composed of discontinuous reinforcement phase beryllium phase and continuous aluminum phase, and is considered to be a beryllium reinforced aluminum-based composite material.
[0003] However, the solidification mode of beryllium aluminum alloy is a typical "volumetric solidification" mode. The wide solidification range determines that defects such as shrinkage cavities and shrinkage will inevitably appear inside the material, which cannot truly reflect the plasticity of aluminum-based composite materials.
[0004] At present, the research focus of beryllium aluminum alloy is on improving the strength, and there has been no significant improvement in the plasticity of beryllium aluminum alloy.
[0005] Therefore, the existing technology needs to be improved. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a high elongation beryllium aluminum alloy and a preparation method thereof. The present invention adopts a method of multiple vacuum melting to fully melt and evenly mix the two metals, beryllium and aluminum, and then quickly pours the beryllium aluminum alloy melt into a water-cooled mold for rapid cooling. The preparation process greatly improves the internal structure density of the beryllium aluminum alloy, thereby improving the elongation (plasticity) of the alloy.
[0007] The first aspect of the present invention provides a method for preparing a high elongation beryllium aluminum alloy, wherein the mass percentage of beryllium in the beryllium aluminum alloy is 60-65wt%, and the balance is aluminum;
[0008] The preparation method comprises the following steps:
[0009] Step S1, placing the pretreated beryllium raw material and aluminum raw material into a melting crucible, and then performing vacuum melting on the beryllium raw material and aluminum raw material for 3 to 5 times to obtain a beryllium aluminum alloy melt;
[0010] Step S2, rapidly pouring the beryllium aluminum alloy melt into a water-cooled mold to cool to room temperature, and obtaining a beryllium aluminum alloy ingot after demoulding;
[0011] The pouring rate is 200-500 g / s, and the temperature of cooling water used in the water-cooled mold is ≤10°C.
[0012] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, in the step S1, after each vacuum melting, the beryllium aluminum alloy melt is naturally cooled to room temperature in the melting crucible to obtain a beryllium aluminum alloy ingot, and the beryllium aluminum alloy ingot is placed in the melting crucible in the opposite direction before the next vacuum melting.
[0013] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, in the step S1, the vacuum melting includes a heat preservation stage after the beryllium raw material and the aluminum raw material are completely melted, and the heat preservation time is 10 to 30 minutes.
[0014] According to the method for preparing high elongation beryllium aluminum alloy according to the first aspect of the present invention, in the step S1, the vacuum degree of the vacuum melting is less than 5.0×10 -3 Pa, the heating power increase rate of the vacuum melting is 10-30kw / min.
[0015] According to the method for preparing high elongation beryllium aluminum alloy according to the first aspect of the present invention, in the step S1, the pretreatment specifically includes:
[0016] Mechanically grinding the beryllium raw material and the aluminum raw material, placing the mechanically ground beryllium raw material and the aluminum raw material into an organic solvent for ultrasonic cleaning and then drying;
[0017] Wherein, the ultrasonic cleaning time is 30 to 60 minutes, the drying temperature is 80 to 100° C., and the drying time is 60 to 90 minutes.
[0018] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, the organic solvent is acetone or ethanol.
[0019] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, in the step S1, the low melting point aluminum raw material is placed at the bottom of the melting crucible, and the high melting point beryllium raw material is placed on the upper layer of the aluminum raw material.
[0020] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, the beryllium raw material and the aluminum raw material are both in the form of flakes or blocks.
[0021] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, the beryllium raw material and the aluminum raw material are placed horizontally.
[0022] According to the method for preparing high elongation beryllium aluminum alloy described in the first aspect of the present invention, the melting crucible can be rotated by ±90°.
[0023] The second aspect of the present invention provides a high elongation beryllium aluminum alloy prepared by the above-mentioned preparation method of high elongation beryllium aluminum alloy, wherein the tensile strength of the beryllium aluminum alloy is 110-120 MPa, the yield strength is 50-60 MPa, and the elongation is 15-20%.
[0024] The solution proposed by the present invention has the following technical effects:
[0025] The invention adopts a preparation process of multiple vacuum melting methods to fully melt and evenly mix beryllium and aluminum metals, and then quickly pours the beryllium aluminum alloy melt into a water-cooled mold for rapid cooling, thereby greatly improving the uniformity and density of the internal structure of the beryllium aluminum alloy, thereby improving the elongation of the alloy.
[0026] In addition, the beryllium aluminum alloy ingot prepared by the method of the present invention has uniform internal structure, good density, and no obvious defects such as shrinkage cavities and shrinkage. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 This is a photograph of the internal structure of the high elongation beryllium aluminum alloy obtained in specific embodiment 1 of the present invention.
[0029] Figure 2 This is a photograph of the internal structure of the high elongation beryllium aluminum alloy obtained in specific embodiment 2 of the present invention.
[0030] Figure 3 This is a photograph of the internal structure of the high elongation beryllium aluminum alloy obtained in specific embodiment 3 of the present invention.
[0031] Figure 4 This is a photograph of the internal structure of the beryllium aluminum alloy obtained in Comparative Example 1.
[0032] Figure 5 This is a photograph of the internal structure of the beryllium aluminum alloy obtained in Comparative Example 2. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] This embodiment provides a method for preparing a high-elongation beryllium aluminum alloy, wherein the mass percentage of beryllium in the beryllium aluminum alloy is 60-65wt%, and the balance is aluminum;
[0035] The preparation method comprises the following steps:
[0036] Step S1, putting the pretreated beryllium raw material and aluminum raw material into a melting crucible, and then performing vacuum melting on the beryllium raw material and aluminum raw material for 3 to 5 times to obtain a beryllium aluminum alloy melt.
[0037] Step S2, rapidly pouring the beryllium aluminum alloy melt into a water-cooled mold to cool to room temperature, and obtaining a beryllium aluminum alloy ingot after demolding.
[0038] In this embodiment, the beryllium and aluminum metals are fully melted and mixed evenly by 3-5 times of vacuum melting to ensure uniform alloy composition, and then the beryllium aluminum alloy melt is quickly poured into a water-cooled mold for rapid cooling. This greatly improves the internal structure density of the beryllium aluminum alloy, thereby improving the elongation of the alloy. In addition, due to the large specific heat capacity of beryllium, if it is slowly cooled, there will be many defects inside the beryllium aluminum alloy.
[0039] At the same time, before vacuum melting, the beryllium raw materials and aluminum raw materials are pretreated to remove surface oxides and surface contamination of the raw materials, ensure the purity of the raw materials, and further reduce defects such as shrinkage cavities and shrinkage pores inside the beryllium aluminum alloy.
[0040] The pouring rate is 200-500 g / s, and the temperature of cooling water used in the water-cooled mold is ≤10°C.
[0041] In this embodiment, when the pouring rate is lower than 200 g / s, the purpose of quickly pouring the melt and quickly cooling the melt cannot be achieved. When the pouring rate is higher than 500 g / s, the gas cannot be discharged in time due to the excessively fast pouring rate, which eventually leads to more pores inside the beryllium aluminum alloy. Therefore, in this embodiment, the pouring rate is controlled at 200-500 g / s.
[0042] The purpose of the present invention is to achieve rapid cooling of the melt, so the temperature of the cooling water cannot be too high. In this embodiment, the temperature of the cooling water is controlled to be less than or equal to 10°C.
[0043] In some embodiments, in the step S1, after each vacuum melting, the beryllium aluminum alloy melt is naturally cooled to room temperature in the melting crucible to obtain a beryllium aluminum alloy ingot, and the beryllium aluminum alloy ingot is placed in the melting crucible in the opposite direction for the next vacuum melting.
[0044] In some embodiments, in the step S1, the vacuum melting includes a heat preservation stage after the beryllium raw material and the aluminum raw material are completely melted, and the heat preservation time is 10 to 30 minutes, so that the alloy solution is suspended in the middle of the crucible and fully stirred and mixed.
[0045] In some embodiments, in step S1, the vacuum degree of the vacuum melting is less than 5.0×10 -3 Pa, the heating power increase rate of the vacuum melting is 10-30kw / min to ensure that the solution is heated evenly and without splashing.
[0046] Preferably, during the vacuum melting heating process, the molten pool conditions are observed from the observation port.
[0047] In some embodiments, in step S1, the preprocessing specifically includes:
[0048] Mechanically grinding the beryllium raw material and the aluminum raw material, placing the mechanically ground beryllium raw material and the aluminum raw material into an organic solvent for ultrasonic cleaning and then drying;
[0049] Wherein, the ultrasonic cleaning time is 30 to 60 minutes, the drying temperature is 80 to 100° C., and the drying time is 60 to 90 minutes.
[0050] Preferably, the organic solvent is acetone or ethanol.
[0051] In some embodiments, in step S1, a low-melting-point aluminum raw material is placed at the bottom of the smelting crucible, and a high-melting-point beryllium raw material is placed on an upper layer of the aluminum raw material.
[0052] Since the bottom temperature of the melting crucible is relatively low, the aluminum raw material with a low melting point is placed at the bottom of the melting crucible, and the beryllium raw material with a high melting point is placed on the upper layer of the aluminum raw material to ensure that the raw materials are fully melted.
[0053] In some embodiments, the purity of the beryllium raw material and the aluminum raw material are both greater than 99%.
[0054] In some embodiments, the beryllium raw material and the aluminum raw material are both in the form of flakes or blocks.
[0055] In some embodiments, the beryllium raw material and the aluminum raw material are placed horizontally to facilitate induction heating.
[0056] In some embodiments, the melting crucible can be rotated by ±90° to facilitate rapid pouring of the beryllium aluminum alloy melt into a water-cooled mold.
[0057] The second aspect of this embodiment provides a high elongation beryllium aluminum alloy prepared by the above-mentioned preparation method of high elongation beryllium aluminum alloy, wherein the tensile strength of the beryllium aluminum alloy is 110-120 MPa, the yield strength is 50-60 MPa, and the elongation is 15-20%.
[0058] Example 1
[0059] The first step is to mechanically polish the beryllium raw material and the aluminum raw material, and then put the mechanically polished beryllium raw material and the aluminum raw material into acetone for ultrasonic cleaning and then drying;
[0060] Among them, the purity of beryllium raw material and aluminum raw material are both greater than 99%, both beryllium raw material and aluminum raw material are in sheet or block shape and placed horizontally, the high melting point beryllium raw material is placed on the upper layer of the aluminum raw material, the mass ratio of beryllium raw material and aluminum raw material is 3:2, the ultrasonic cleaning time is 30 minutes, the drying temperature is 80°C, and the drying time is 60 minutes.
[0061] In the second step, the pre-treated beryllium raw material and aluminum raw material are placed in a melting crucible and vacuumed to 5.0×10 -3 Pa, vacuum melting is started, and the heating power increase rate of vacuum melting is set to 20kw / min, until the beryllium raw material and the aluminum raw material are completely melted, and the heating is stopped after 10-30min of heat preservation, so that the beryllium aluminum alloy melt is naturally cooled to room temperature in the melting crucible to obtain a beryllium aluminum alloy ingot, and the beryllium aluminum alloy ingot is placed in the melting crucible in the opposite direction before the next vacuum melting. A total of 3 vacuum meltings are performed to obtain the beryllium aluminum alloy melt to be cast.
[0062] The third step is to quickly pour the beryllium aluminum alloy melt to be poured into a water-cooled mold to cool it to room temperature, and then demold it to obtain a beryllium aluminum alloy ingot;
[0063] Among them, the pouring rate is 200g / s, and the temperature of cooling water used in the water-cooled mold is 5±3℃.
[0064] The chemical composition and mechanical properties of the beryllium aluminum alloy ingot obtained in Example 1 were tested. According to the test, the mass percentage of beryllium in the beryllium aluminum alloy ingot was 59.9%, the mass percentage of aluminum was 40.1%, the tensile strength was 112.5 MPa, the yield strength was 52.6 MPa, and the elongation was 15.2%.
[0065] like Figure 1 As shown, the internal structure of the beryllium aluminum alloy ingot prepared in Example 1 is uniform, compact, and has no obvious defects such as shrinkage cavities and shrinkage.
[0066] Example 2
[0067] The difference from Example 1 is that the mass ratio of beryllium raw material to aluminum raw material is 62:38, the time for ultrasonic cleaning is 45 minutes, the drying temperature is 90°C, and the drying time is 80 minutes; the heating power increase rate of vacuum melting is 10kw / min, and a total of 4 vacuum meltings are performed; the pouring rate is 300g / s, and the temperature of cooling water used for the water-cooled mold is 6±3°C.
[0068] The chemical composition and mechanical properties of the beryllium aluminum alloy ingot obtained in Example 2 were tested. According to the test, the mass percentage of beryllium in the beryllium aluminum alloy ingot was 61.9%, the mass percentage of aluminum was 38.1%, the tensile strength was 115.3 MPa, the yield strength was 56.2 MPa, and the elongation was 18.1%.
[0069] like Figure 2 As shown, the internal structure of the beryllium aluminum alloy ingot prepared in Example 2 is uniform, compact, and has no obvious defects such as shrinkage cavities and shrinkage.
[0070] Example 3
[0071] The difference from Example 1 is that the mass ratio of beryllium raw material to aluminum raw material is 65:35, the ultrasonic cleaning time is 60 min, the drying temperature is 100°C, and the drying time is 90 min; the heating power increase rate of vacuum melting is 30 kw / min, and a total of 5 vacuum meltings are performed; the pouring rate is 400 g / s, and the temperature of the cooling water used for the water-cooled mold is 4±3°C.
[0072] The chemical composition and mechanical properties of the beryllium aluminum alloy ingot obtained in Example 3 were tested. According to the test, the mass percentage of beryllium in the beryllium aluminum alloy ingot was 64.8%, the mass percentage of aluminum was 35.2%, the tensile strength was 119.8 MPa, the yield strength was 59.7 MPa, and the elongation was 20.0%.
[0073] like Figure 3 As shown, the internal structure of the beryllium aluminum alloy ingot prepared in Example 3 is uniform, compact, and has no obvious defects such as shrinkage cavities and shrinkage.
[0074] Comparative Example 1
[0075] The difference from Example 1 is that vacuum melting is performed twice in total; the pouring rate is 150 g / s, and the temperature of cooling water used in the water-cooled mold is 25±3°C.
[0076] The chemical composition and mechanical properties of the beryllium aluminum alloy ingot obtained in Comparative Example 1 were tested. According to the test, the mass percentage of beryllium in the beryllium aluminum alloy ingot was 60.1%, the mass percentage of aluminum was 39.9%, the tensile strength was 92.1 MPa, the yield strength was 41.6 MPa, and the elongation was 1.9%.
[0077] like Figure 4 As shown, the internal structure of the beryllium aluminum alloy ingot prepared in Comparative Example 1 has obvious defects such as shrinkage cavities and shrinkage.
[0078] Comparative Example 2
[0079] The difference from Example 1 is that vacuum melting is performed twice in total; the pouring rate is 600 g / s, and the temperature of cooling water used in the water-cooled mold is 25±3°C.
[0080] The chemical composition and mechanical properties of the beryllium aluminum alloy ingot obtained in Comparative Example 2 were tested. According to the test, the mass percentage of beryllium in the beryllium aluminum alloy ingot was 60.2%, aluminum was 39.8%, the tensile strength was 79.8 MPa, the yield strength was 40.1 MPa, and the elongation was 1.5%.
[0081] like Figure 5 As shown, the internal structure of the beryllium aluminum alloy ingot prepared in Comparative Example 2 has obvious defects such as shrinkage cavities and shrinkage.
[0082] In summary, the solution proposed by the present invention has the following technical effects:
[0083] The invention adopts a preparation process of multiple vacuum melting methods to fully melt and evenly mix beryllium and aluminum metals, and then quickly pours the beryllium aluminum alloy melt into a water-cooled mold for rapid cooling, thereby greatly improving the uniformity and density of the internal structure of the beryllium aluminum alloy, thereby improving the elongation of the alloy.
[0084] In addition, the beryllium aluminum alloy ingot prepared by the method of the present invention has uniform internal structure, good density, and no obvious defects such as shrinkage cavities and shrinkage.
[0085] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.
Claims
1. A method for preparing a high elongation beryllium aluminum alloy, characterized in that: The mass percentage of beryllium in the beryllium aluminum alloy is 60-65wt%, and the balance is aluminum; The preparation method comprises the following steps: Step S1, placing the pretreated beryllium raw material and aluminum raw material into a melting crucible, and then performing vacuum melting on the beryllium raw material and aluminum raw material for 3 to 5 times to obtain a beryllium aluminum alloy melt; Step S2, rapidly pouring the beryllium aluminum alloy melt into a water-cooled mold to cool to room temperature, and obtaining a beryllium aluminum alloy ingot after demoulding; The pouring rate is 200-500 g / s, and the temperature of cooling water used in the water-cooled mold is ≤10°C.
2. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: In the step S1, after each vacuum melting, the beryllium aluminum alloy melt is naturally cooled to room temperature in the melting crucible to obtain a beryllium aluminum alloy ingot, and the beryllium aluminum alloy ingot is placed in the melting crucible in the opposite direction for the next vacuum melting.
3. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: In the step S1, the vacuum melting includes a heat preservation stage after the beryllium raw material and the aluminum raw material are completely melted, and the heat preservation time is 10 to 30 minutes.
4. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: In step S1, the vacuum degree of the vacuum melting is less than 5.0×10 -3 Pa, the heating power increase rate of the vacuum melting is 10-30kw / min.
5. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: In step S1, the preprocessing specifically includes: Mechanically grinding the beryllium raw material and the aluminum raw material, placing the mechanically ground beryllium raw material and the aluminum raw material into an organic solvent for ultrasonic cleaning and then drying; Wherein, the ultrasonic cleaning time is 30 to 60 minutes, the drying temperature is 80 to 100° C., and the drying time is 60 to 90 minutes.
6. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: In the step S1, a low-melting-point aluminum raw material is placed at the bottom of the smelting crucible, and a high-melting-point beryllium raw material is placed on the upper layer of the aluminum raw material.
7. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: The beryllium raw material and the aluminum raw material are both in the form of flakes or blocks.
8. The method for preparing high elongation beryllium aluminum alloy according to claim 7, characterized in that: The beryllium raw material and the aluminum raw material are placed horizontally.
9. The method for preparing high elongation beryllium aluminum alloy according to claim 1, characterized in that: The melting crucible can be rotated by ±90°.
10. A high elongation beryllium aluminum alloy prepared by the method for preparing a high elongation beryllium aluminum alloy according to any one of claims 1 to 9, characterized in that: The tensile strength of the beryllium aluminum alloy is 110-120 MPa, the yield strength is 50-60 MPa, and the elongation is 15-20%.
Citation Information
Cited By
High-elongation beryllium-aluminum alloy and preparation method therefor
WO2025252256A1