Preparation method of semiconductor structure and semiconductor structure

By introducing a nitride dielectric layer during the fabrication of dynamic random access memory, the problem of poor electrical stability caused by transistor damage is solved, better protection and etching control are achieved, and the stability of the device is improved.

CN118900558AActive Publication Date: 2024-11-05CHANGXIN MEMORY TECH INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310483888.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-05
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

During the fabrication of dynamic random access memory (DRAM), transistors are easily damaged, resulting in poor electrical stability of the device.

Method used

A nitrided dielectric layer is introduced during the fabrication process. The oxide dielectric layer is transformed into a nitrided dielectric layer through remote plasma nitriding treatment to form a nitrided dielectric layer to protect the active region. It also serves as an etching stop layer during the etching process to reduce oxidation damage and over-etching damage in the active region.

Benefits of technology

It effectively protects the active region, reduces damage during the fabrication process, and improves the electrical stability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900558A_ABST
    Figure CN118900558A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a semiconductor device structure and a semiconductor structure. The preparation method of the semiconductor structure comprises the following steps: providing a semiconductor substrate, wherein the semiconductor substrate comprises an active region; forming a gate structure on the active region; nitriding the surface of the active region which is not covered by the gate structure to form a nitriding dielectric layer, and then preparing a lightly doped drain region in the active region below the nitriding dielectric layer; forming a side wall structure on the side wall of the gate structure; and preparing a source-drain region in the active region which is not covered by the gate structure and the side wall structure. The preparation method of the semiconductor structure can effectively improve the damage to the transistor in the preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for preparing a semiconductor structure and a semiconductor structure. Background Art

[0002] Dynamic Random Access Memory (DRAM) is a commonly used semiconductor memory device. Usually, a DRAM wafer includes an array area and a peripheral area, and a circuit including transistors is arranged in the peripheral area. Among them, the transistors in the peripheral area are easily damaged during the preparation process, resulting in poor electrical stability of the device. Summary of the invention

[0003] Based on this, it is necessary to provide a method for preparing a semiconductor structure to address the problems in the above-mentioned background technology, so as to improve the damage suffered by the transistor during the preparation process and enhance the electrical stability of the device.

[0004] According to some embodiments of the present disclosure, a method for preparing a semiconductor structure is provided, comprising the following steps:

[0005] Providing a semiconductor substrate, the semiconductor substrate comprising an active region;

[0006] forming a gate structure on the active area;

[0007] Performing nitridation treatment on the surface of the active area not covered by the gate structure to form a nitrided dielectric layer, and then preparing a lightly doped drain region in the active area under the nitrided dielectric layer;

[0008] forming a sidewall structure on the sidewall of the gate structure;

[0009] A source and drain region is prepared in the active region not covered by the gate structure and the spacer structure.

[0010] In some embodiments of the present disclosure, before the nitridation treatment is performed, the surface of the active area not covered by the gate structure has an oxidized dielectric layer;

[0011] During the nitridation treatment, the oxidized dielectric layer is transformed into the nitrided dielectric layer.

[0012] In some embodiments of the present disclosure, the nitridation treatment includes: using a reaction gas to transform the oxidized dielectric layer into the nitrided dielectric layer in a remote plasma nitridation treatment, wherein the reaction gas includes a nitrogen source gas and a reducing gas.

[0013] In some embodiments of the present disclosure, in the reaction gas, a flow ratio of the nitrogen source gas to the reducing gas is 1:0.5 to 1:3.

[0014] In some embodiments of the present disclosure, during the nitridation process, the reaction temperature is controlled to be 30°C to 60°C.

[0015] In some embodiments of the present disclosure, during the nitridation process, the reaction time is controlled to be 30s to 180s.

[0016] In some embodiments of the present disclosure, during the nitridation process, the thickness of the formed nitrided dielectric layer is controlled to be 5 nm to 30 nm.

[0017] In some embodiments of the present disclosure, forming a gate structure on the active area includes:

[0018] A gate material layer is formed on the semiconductor substrate, and the gate material layer is etched to form the gate structure.

[0019] In some embodiments of the present disclosure, after forming the gate structure and before performing the nitridation treatment, the method further includes:

[0020] forming a first protective layer, wherein the first protective layer covers a surface of the gate structure and a surface of the active area not covered by the gate structure;

[0021] forming a second protective layer, wherein the second protective layer covers the surface of the first protective layer;

[0022] Etching the second protection layer and the first protection layer covering the surface of the active area to expose the active area not covered by the gate structure; and,

[0023] The second protection layer on the sidewall of the gate structure is removed and at least the first protection layer covering the sidewall of the gate structure is retained.

[0024] In some embodiments of the present disclosure, the material of the first protective layer is different from the material of the oxidizing medium layer, and the material of the first protective layer includes nitride; and / or,

[0025] The material of the second protection layer is different from that of the first protection layer, and the material of the second protection layer includes oxide.

[0026] In some embodiments of the present disclosure, forming a spacer structure on the sidewall of the gate structure includes:

[0027] forming a spacer material layer, wherein the spacer material layer covers the surface of the first protective layer and the nitride dielectric layer;

[0028] The sidewall material layer on the nitride dielectric layer is etched using the nitride dielectric layer as an etch stop layer, and a portion of the sidewall material layer on both sides of the gate structure is retained to serve as the sidewall structure.

[0029] In some embodiments of the present disclosure, after preparing the spacer structure, the method further includes: preparing a third protective layer covering the spacer structure.

[0030] In some embodiments of the present disclosure, after preparing the source and drain regions, a step of preparing source and drain contacts on the source and drain regions is also included.

[0031] In some embodiments of the present disclosure, the step of preparing source-drain contacts includes:

[0032] forming an interlayer dielectric layer on the semiconductor substrate, and forming a connection hole in the interlayer dielectric layer with the bottom exposing the source and drain regions;

[0033] The connection hole is filled with a conductive material electrically connected to the source and drain regions to form the source and drain contacts.

[0034] Furthermore, according to some embodiments of the present disclosure, there is also provided a semiconductor structure, comprising:

[0035] An active region, wherein a lightly doped drain region and a source-drain region are disposed in the active region;

[0036] A gate structure, wherein the gate structure is disposed on the active area;

[0037] A sidewall structure, wherein the sidewall structure is disposed on a sidewall of the gate structure;

[0038] A nitride dielectric layer is disposed between the sidewall structure and the active area.

[0039] In the conventional technology, when preparing the sidewall structure, the surface of the active area usually has an oxidizing dielectric layer. However, when preparing the sidewall structure, the oxidizing dielectric layer cannot effectively prevent the deposited raw materials from reacting with the active area, resulting in oxidation damage to the active area. In addition, the etching progress when preparing the sidewall structure is difficult to accurately control, which easily leads to over-etching, resulting in over-etching damage to the active area.

[0040] In the method for preparing the semiconductor structure provided by the present disclosure, a step of nitriding the surface of the active area to form a nitride dielectric layer is introduced between forming the gate structure and forming the sidewall structure. Compared with the oxidized dielectric layer used in the conventional technology, when preparing the sidewall structure, the nitride dielectric layer can protect the active area from oxidation damage, and the etching rate of the nitride dielectric layer is easier to control, so it is more conducive to protecting the active area and improving the over-etching damage of the active area. Therefore, the method for preparing the semiconductor structure can effectively improve the damage suffered by the transistor during the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 A schematic diagram of the steps of a method for preparing a semiconductor structure disclosed in the present invention;

[0042] Figure 2 A schematic diagram of a cross-sectional structure of a semiconductor substrate provided by the present disclosure;

[0043] Figure 3 For Figure 2 A schematic diagram of a structure for preparing a gate structure based on the structure shown;

[0044] Figure 4 For Figure 3 A schematic diagram of a structure for preparing a first protective layer and a second protective layer based on the structure shown;

[0045] Figure 5 For Figure 4 A schematic diagram of a structure in which a second protective layer and a first protective layer on the active area are etched based on the structure shown;

[0046] Figure 6 For Figure 5 A schematic diagram of a structure in which the second protective layer is removed based on the structure shown;

[0047] Figure 7 For Figure 6 A schematic diagram of a structure in which a nitrided dielectric layer is prepared by nitridation treatment based on the structure shown;

[0048] Figure 8 For Figure 7 A schematic diagram of a structure for preparing a lightly doped drain region based on the structure shown;

[0049] Fig. 9 For Figure 8 A schematic diagram of a structure for preparing a sidewall material layer based on the structure shown;

[0050] Fig.10 For Fig. 9 A schematic diagram of a structure for preparing a side wall structure based on the structure shown;

[0051] Fig.11 For Fig.10 A schematic diagram of a structure for preparing source and drain regions based on the structure shown;

[0052] Fig.12 For Fig.11 A schematic diagram of a structure for preparing a third protective layer based on the structure shown;

[0053] Fig.13 For Fig.12 A schematic diagram of a structure in which a first interlayer dielectric layer, a second interlayer dielectric layer, a first pattern layer and a second pattern layer are sequentially stacked on the basis of the structure shown;

[0054] Fig.14 For Fig.13 A schematic diagram of a structure in which a second pattern layer, a first pattern layer, a second interlayer dielectric layer and a first interlayer dielectric layer are etched on the basis of the structure shown;

[0055] Fig.15 For Fig.14 A schematic diagram of a structure for preparing a third pattern layer and a fourth pattern layer based on the structure shown;

[0056] Fig.16 For Fig.15 A schematic diagram of a structure in which a fourth pattern layer, a third pattern layer, a second interlayer dielectric layer, a third protection layer and a gate top protection layer are etched on the basis of the structure shown;

[0057] Fig.17 For Fig.16 A schematic diagram of a structure in which the third pattern layer and the fourth pattern layer are removed from the structure shown;

[0058] Fig.18 For Fig.17 A schematic diagram of a structure for preparing source-drain contacts and gate leads based on the structure shown;

[0059] The reference numerals and their meanings are as follows:

[0060] 100, active area; 110, oxide dielectric layer; 120, nitride dielectric layer; 130, source and drain area; 140, lightly doped drain area; 150, inversion doped area; 200, gate structure; 201, first gate conductive layer; 202, gate barrier layer; 203, second gate conductive layer; 210, gate protection layer; 220, first protection layer; 230, sidewall structure; 231, sidewall material layer; 240, third protection layer; 250, first interlayer dielectric layer; 260, second interlayer dielectric layer; 310, second protection layer; 320, first pattern layer; 330, second pattern layer; 340, third pattern layer; 350, fourth pattern layer; 410, source and drain contacts; 420, gate lead. DETAILED DESCRIPTION

[0061] In order to facilitate understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are shown in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thorough and comprehensive.

[0062] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0063] It should be understood that when an element or layer is referred to as being "on, adjacent to, connected to or coupled to other elements or layers, it may be directly on, adjacent to, connected to or coupled to other elements or layers, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on, directly adjacent to, directly connected to or directly coupled to other elements or layers, there may be no intervening elements or layers. It should be understood that, although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below may be represented as a second element, component, region, layer or part.

[0064] Spatially relative terms such as "under," "below," "below," "under," "above," "above," etc., may be used herein for ease of description to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that in addition to the orientations shown in the figures, the spatially relative terms are intended to include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, then the elements or features described as "under other elements" or "under" or "under" will be oriented as "on" the other elements or features. Therefore, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be oriented otherwise (rotated 90 degrees or other orientations) and the spatial descriptors used herein are interpreted accordingly.

[0065] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be a limitation of the present disclosure. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0066] The disclosed embodiments are described herein with reference to cross-sectional views which are schematic diagrams of ideal embodiments (and intermediate structures) of the present disclosure. As such, variations from the shapes shown due to, for example, manufacturing techniques and / or tolerances can be expected. Therefore, the embodiments of the present disclosure should not be limited to the specific shapes of the regions shown herein, but rather include shape deviations due to, for example, manufacturing, and the regions shown in the figures are schematic in nature, and their shapes are not intended to show the actual shapes of the regions of the device and are not intended to limit the scope of the present disclosure.

[0067] The present disclosure Figure 1 A method for preparing a semiconductor structure according to the above embodiment is shown. Figure 1 As shown, the method for preparing the semiconductor structure includes steps S1 to S8, which are specifically as follows.

[0068] Step S1, providing a semiconductor substrate.

[0069] Figure 2 FIG. 4 shows a schematic diagram of the cross-sectional structure of the semiconductor substrate. Figure 2 As shown, the semiconductor substrate includes an active region 100 and an oxidized dielectric layer 110 . The oxidized dielectric layer 110 is stacked on the active region 100 , and the oxidized dielectric layer 110 completely covers the surface of the active region 100 .

[0070] It can be understood that the material of the oxidized dielectric layer 110 includes oxide. In some examples of this embodiment, the material of the oxidized dielectric layer 110 can be an insulating material.

[0071] In some examples of this embodiment, the material of the active region 100 may be a semiconductor material. For example, the material of the active region 100 may include one or more of silicon, germanium, and a silicon-germanium alloy. Further, the material of the active region 100 may also include a doping element.

[0072] In some examples of this embodiment, the material of the oxidized dielectric layer 110 may include an oxide of the material of the active region 100. For example, if the material of the active region 100 includes silicon, the material of the oxidized dielectric layer 110 may include silicon oxide. The oxidized dielectric layer 110 may be formed by oxidation based on the material of the active region 100, or may be prepared by deposition.

[0073] In some examples of this embodiment, the thickness of the oxidizing medium layer 110 may be 5 nm to 100 nm. Further, the thickness of the oxidizing medium layer 110 may be appropriately thinner, for example, the thickness of the oxidizing medium layer 110 may be 5 nm, 10 nm, 20 nm, 30 nm or 50 nm. The thickness of the oxidizing medium layer 110 may also be in a range between any two thicknesses.

[0074] Step S2, forming a gate structure on the active area.

[0075] Figure 3 Shown in Figure 2 A schematic diagram of a structure of preparing a gate structure 200 based on the structure shown in FIG. Figure 3 As shown, the gate structure 200 is disposed on a side of the oxide dielectric layer 110 away from the active area 100, and the gate structure 200 is disposed on a portion of the active area 100. For ease of description, in this embodiment, the portion of the active area 100 located under the gate structure 200 is recorded as the gate region of the active area 100.

[0076] Reference Figure 3 As shown, there is an oxide dielectric layer 110 between the gate structure 200 and the active area 100. The oxide dielectric layer 110 can be used as a gate dielectric for insulating the gate structure 200 and the active area 100.

[0077] In some examples of this embodiment, reference Figure 3 As shown, the gate structure 200 includes a first gate conductive layer 201, a gate barrier layer 202 and a second gate conductive layer 203 which are stacked in sequence from bottom to top.

[0078] In some examples of this embodiment, the material of the first gate conductive layer 201 may be a conductor and / or semiconductor material having high adhesion to the oxidized dielectric layer 110. In this embodiment, the material of the first gate conductive layer 201 may include polysilicon. Further, the polysilicon is doped polysilicon to make the first gate conductive layer 201 have better conductivity.

[0079] In some examples of this embodiment, the material of the second gate conductive layer 203 may be a conductor material with good conductivity, so that the gate structure 200 as a whole has good conductivity. For example, the material of the second gate conductive layer 203 may be a metal material. Further, the material of the second gate conductive layer 203 may include one or more of gold, silver, copper, aluminum and tungsten. In this embodiment, the material of the second gate conductive layer 203 is tungsten.

[0080] The gate barrier layer 202 is disposed between the first gate conductive layer 201 and the second gate conductive layer 203, and is used to prevent the elements of the second gate conductive layer 203 from diffusing into the first gate conductive layer 201. In some examples of this embodiment, the material of the gate barrier layer 202 may include one or more of titanium and titanium nitride. In this embodiment, the material of the gate barrier layer 202 is titanium nitride.

[0081] Reference Figure 3 As shown, in some examples of this embodiment, during or after the step of preparing the gate structure 200, a step of preparing a gate top protection layer 210 is also included. The gate top protection layer 210 is disposed on a side of the gate structure 200 away from the semiconductor substrate.

[0082] In some examples of this embodiment, the material of the gate top protection layer 210 may include one or more of silicon nitride, silicon oxide, and silicon oxynitride. In this embodiment, the material of the gate top protection layer 210 is silicon nitride.

[0083] Among them, the steps of preparing the gate structure 200 and the gate top protection layer 210 may include: preparing a first conductive material layer, a blocking material layer, a second conductive material layer and a top protection material layer in sequence on a semiconductor substrate, and then etching to remove the top protection material layer, the second conductive material layer, the blocking material layer and the first conductive material layer on other areas outside the gate area to respectively form a gate top protection layer 210, a second gate conductive layer 203, a gate blocking layer 202 and a first gate conductive layer 201.

[0084] Step S3, preparing a first protection layer covering the gate structure.

[0085] The first protection layer 220 is used to protect the gate structure 200 .

[0086] In some examples of this embodiment, after forming the gate structure 200, it also includes: forming a first protective layer 220, the first protective layer 220 covers the surface of the gate structure 200 and the surface of the active area 100 not covered by the gate structure 200; forming a second protective layer 310, the second protective layer 310 covers the surface of the first protective layer 220; etching the second protective layer 310 and the first protective layer 220 covering the surface of the active area 100 to expose the active area 100 not covered by the gate structure 200; and removing the second protective layer 310 on the side wall of the gate structure 200 and at least retaining the first protective layer 220 covering the side wall of the gate structure 200.

[0087] Figure 4 Shown in Figure 3 A schematic diagram of the structure of preparing the first protective layer 220 and the second protective layer 310 based on the structure shown in FIG. Figure 4 As shown, the first protective layer 220 covers the gate structure 200 and the oxidized dielectric layer 110 that is not shielded by the gate structure 200. In the actual preparation process, the first protective layer 220 can be directly prepared by deposition on the surface of the semiconductor substrate and the gate structure 200. The second protective layer 310 is prepared on the first protective layer 220. In the actual preparation process, the second protective layer 310 can be prepared by deposition on the surface of the first protective layer 220.

[0088] Figure 5 Shown in Figure 4 FIG. 1 is a schematic diagram of a structure in which the second protection layer 310 and the first protection layer 220 on the active area 100 are etched based on the structure shown.

[0089] Reference Figure 5 As shown, in some examples of this embodiment, in the step of etching the second protective layer 310 and the first protective layer 220 on the active area 100, the second protective layer 310 and the first protective layer 220 stacked on the oxidized dielectric layer 110 are removed, while a portion of the first protective layer 220 attached to the side wall of the gate structure 200 is retained.

[0090] It can be understood that after the second protection layer 310 and the first protection layer 220 are removed, the oxide dielectric layer 110 is exposed from the area outside the gate structure.

[0091] In some examples of this embodiment, the second protective layer 310 and the first protective layer 220 may be removed by dry etching. Further, by dry etching in a direction perpendicular to the semiconductor substrate, the second protective layer 310 and the first protective layer 220 stacked on the oxidizing medium layer 110 can be removed, while retaining the first protective layer 220 attached to the sidewall of the gate structure 200.

[0092] In addition, refer to Figure 5 As shown, during the etching process using this method, the second protection layer 310 and the first protection layer 220 located above the gate structure 200 will also be etched simultaneously, but this will basically not affect the first protection layer 220 attached to the side wall of the gate structure 200.

[0093] The first protective layer 220 attached to the sidewall of the gate structure 200 is used to protect the gate structure 200 in subsequent processes. In some examples of this embodiment, the material of the first protective layer 220 includes an insulating material. For example, the material of the first protective layer 220 may include one or more of silicon nitride, silicon oxide, and silicon oxynitride. In this embodiment, the material of the first protective layer 220 is silicon nitride.

[0094] In some examples of this embodiment, the material of the second protective layer 310 includes an insulating material. For example, the material of the second protective layer 310 may include one or more of silicon nitride, silicon oxide, and silicon oxynitride. In this embodiment, the material of the second protective layer 310 is silicon oxide.

[0095] In some examples of this embodiment, during the etching of the second protective layer 310, the first protective layer 220 may be used as an etching stop layer to control the etching amount of the second protective layer 310. Therefore, in this embodiment, the material of the first protective layer 220 may be different from the material of the second protective layer 310, so that the second protective layer 310 and the first protective layer 220 have different etching rates.

[0096] In some examples of this embodiment, during the etching of the first protective layer 220, the oxidizing medium layer 110 may be used as an etching stop layer to control the etching amount of the first protective layer 220. Therefore, in this embodiment, the material of the first protective layer 220 may be different from the material of the oxidizing medium layer 110, so that the first protective layer 220 and the oxidizing medium layer 110 have different etching rates.

[0097] Figure 6 Shown in Figure 5 The schematic diagram of the structure shown in FIG. 1 is a schematic diagram of a structure in which the second protective layer 310 is removed from the structure shown in FIG. Figure 6 As shown, a portion of the second protection layer 310 originally attached to the sidewall of the gate structure 200 is removed.

[0098] In some examples of this embodiment, the second protection layer 310 may be removed by cleaning, which can remove the second protection layer 310 remaining on the sidewall without substantially affecting the first protection layer 220 .

[0099] Understandably, through Figures 4 to 6In this way, the first protection layer 220 can be prepared on the side wall of the gate structure 200 to protect the side wall of the gate structure 200.

[0100] Step S4, performing nitridation treatment on the surface of the active area not covered by the gate structure to form a nitrided dielectric layer.

[0101] The nitride dielectric layer is used to protect the surface of the active area 100 .

[0102] In some examples of this embodiment, reference Figure 6 As shown, before the nitridation treatment, the surface of the active area 100 not covered by the gate structure 200 has an oxidized dielectric layer 110 . During the nitridation treatment, the oxidized dielectric layer 110 can be transformed into a nitrided dielectric layer 120 .

[0103] It can be understood that in this embodiment, the oxidizing medium layer 110 is provided on the surface of the active region 100 in advance and is retained until this step, but in some other embodiments, the oxidizing medium layer can also be formed by natural oxidation after the surface of the active region is exposed.

[0104] Figure 7 Shown in Figure 6 A schematic diagram of a structure of a nitrided dielectric layer 120 prepared by nitridation treatment on the basis of the structure shown in FIG. Figure 7 As shown, the portion of the oxidized dielectric layer 110 on the active area 100 that is not covered by the gate structure 200 is transformed into the nitride dielectric layer 120, so the nitride dielectric layer 120 also shields the active area 100 that is not covered by the gate structure 200. It can be understood that in this step, the oxidized dielectric layer 110 that is not shielded by the gate structure 200 can be transformed into the nitride dielectric layer 120, and the oxidized dielectric layer 110 shielded by the gate structure 200 can be retained to be used as a gate dielectric.

[0105] The nitride dielectric layer 120 is transformed from the oxidized dielectric layer 110, which means that the oxygen element in the oxidized dielectric layer 110 is at least partially replaced by the nitrogen element to serve as the nitride dielectric layer 120, that is, the nitride dielectric layer 120 may still contain a portion of oxide. In some examples of this embodiment, in the step of reacting the oxidized dielectric layer 110 to form the nitride dielectric layer 120, all the oxygen elements in the oxidized dielectric layer 110 are replaced by the nitrogen element, which means that the nitride dielectric layer 120 does not contain the oxygen element.

[0106] In some examples of this embodiment, the nitridation process includes: using a reaction gas to transform the oxidized dielectric layer 110 into a nitrided dielectric layer 120 in a remote plasma nitridation process, and the reaction gas may include a nitrogen source gas and a reducing gas. Figure 7 As shown, Figure 7The dotted arrow in shows the moving direction of the plasma of the reaction gas. After the oxide dielectric layer 110 which is not shielded by the gate structure 200 contacts the plasma of the reaction gas, a nitridation reaction occurs and a nitrided dielectric layer 120 is formed.

[0107] The nitrogen source gas may be a raw material that can react with the material of the oxidizing medium layer 110 to form a corresponding nitride. The reducing gas is used to reduce the oxidizing medium layer 110 during the nitridation process to promote the reaction.

[0108] In some examples of this embodiment, the nitrogen source may include nitrogen gas.

[0109] In some examples of this embodiment, the reducing gas may be hydrogen.

[0110] In some examples of this embodiment, during the nitridation process, the flow ratio of nitrogen to reducing gas is (1:0.5) to (1:3). Further, in the reaction gas, the flow ratio of nitrogen to reducing gas is (1:0.5) to (1:2).

[0111] In some examples of this embodiment, during the nitridation process, the reaction temperature can be controlled to be 30° C. to 60° C.

[0112] In some examples of this embodiment, during the nitridation process, the reaction time can be controlled to be 30s to 180s.

[0113] In some examples of this embodiment, the thickness of the formed nitride dielectric layer 120 may be controlled to be 5 nm to 30 nm.

[0114] Among them, the nitride dielectric layer 120 can not only prevent the active area 100 from being damaged due to oxidation of elements in the active area 100. Furthermore, compared with the active area 100 and the oxide dielectric layer 110, the nitride dielectric layer 120 is more difficult to be etched in the subsequent process, and thus can be used as an etching stop layer in the subsequent process to effectively protect the active area 100 located below, thereby further improving the damage caused by etching of the active area 100.

[0115] Step S5, preparing a lightly doped drain region in the active region under the nitride dielectric layer.

[0116] Figure 8 Shown in Figure 7 Schematic diagram of the structure for preparing a lightly doped drain region based on the structure shown.

[0117] Reference Figure 8As shown, the lightly doped drain region 140 is located in the active region 100 not covered by the gate structure 200, and the doping type of the lightly doped drain region 140 may be the same as the doping type of the active region 100. The lightly doped drain region 140 is also called a low-dose doped drain region (Lightly Doped Drain, LDD), which may be located at the edge of the gate close to the channel, and its doping concentration is lower than the doping concentration of the source and drain regions prepared subsequently, and its function is to provide a doping concentration gradient for the source and drain regions.

[0118] Reference Figure 8 As shown, in some examples of this embodiment, after forming the nitride dielectric layer 120, a step of preparing an inversion doping region 150 in the active region under the nitride dielectric layer is also included. The inversion doping region 150 can be located below the lightly doped drain region 140, and the doping type of the inversion doping region 150 is opposite to the doping type of the active region 100. The inversion doping region 150 can serve as a halo in the semiconductor structure, and the inversion element in the inversion doping region 150 can inhibit the depletion layer of the source and drain from diffusing into the channel to form a charge sharing effect, prevent the penetration of the source and drain, and reduce the leakage current and threshold drift.

[0119] In some examples of this embodiment, the lightly doped drain region 140 may be prepared by ion implantation.

[0120] In some examples of this embodiment, the inversion doping region 150 may also be prepared by ion implantation.

[0121] It can be understood that by controlling the energy of the ion implantation, the depth of the ion implantation can be controlled so that the lightly doped drain region 140 and the inversion doped region 150 are located at different depths in the active region 100 .

[0122] Step S6, forming a spacer structure on the sidewall of the gate structure.

[0123] In some examples of this embodiment, the step of forming a sidewall structure on the sidewall of the gate structure includes: forming a sidewall material layer, the sidewall material layer covering the surface of the first protective layer 220 and the nitride dielectric layer 120, etching the sidewall material layer located on the nitride dielectric layer 120 using the nitride dielectric layer 120 as an etching stop layer, and retaining part of the sidewall material layer on both sides of the gate structure 200 as a sidewall structure.

[0124] Fig. 9 Shown in Figure 8 A schematic diagram of a structure for preparing a spacer material layer 231 based on the structure shown in FIG. Fig. 9 As shown, the spacer material layer 231 entirely covers the surfaces of the first protection layer 220 and the nitride dielectric layer 120 .

[0125] In some examples of this embodiment, the material of the spacer material layer 231 may include one or more of silicon oxide and silicon oxynitride. In this embodiment, the material of the spacer material layer 231 is silicon oxide.

[0126] In some examples of this embodiment, the spacer material layer 231 may be prepared by chemical vapor deposition.

[0127] Fig.10 Shown in Fig. 9 A schematic diagram of a structure of preparing a sidewall structure 230 based on the structure shown in FIG. Fig.10 As shown, in this embodiment, the spacer structure 230 can cover the lightly doped drain region 140. In the step of preparing the spacer structure 230, the spacer material layer 231 located on the nitride dielectric layer 120 is etched using the nitride dielectric layer 120 as an etch stop layer, and a portion of the spacer material layer 231 on both sides of the gate structure 200 is retained as the spacer structure 230.

[0128] In some examples of this embodiment, when etching the spacer material layer 231, the entire spacer material layer 231 can be etched at the same time. During the etching process, the spacer material layer 231 located on the lightly doped drain region 140 is thicker. When the spacer material layer 231 on the active region 100 outside the lightly doped drain region 140 is completely removed, most of the spacer material layer 231 located on the lightly doped drain region 140 can be retained and used as the spacer structure 230.

[0129] In some examples of this embodiment, the material of the spacer material layer 231 can be different from the material of the nitride dielectric layer 120, so that the nitride dielectric layer 120 can be used as an etching stop layer. During the etching process, an etchant with a higher etching rate for the spacer material layer 231 than for the nitride dielectric layer 120 can be selected. For example, the etching selectivity ratio of the etchant for the spacer material layer 231 and the nitride dielectric layer 120 is ≥10:1.

[0130] Reference Fig.10 As shown, after part of the spacer material layer 231 is removed, part of the nitride dielectric layer 120 is exposed from the area outside the spacer structure 230. In some examples of this embodiment, after the step of preparing the spacer structure 230, a step of removing the nitride dielectric layer 120 exposed from the area outside the spacer structure 230 is also included. The method of removing the nitride dielectric layer 120 can be dry etching.

[0131] In some examples of this embodiment, no additional mask may be required in the step of removing the nitride dielectric layer 120. It is understood that when removing the nitride dielectric layer 120 on the source / drain region, the spacer structure 230 and the gate top protection layer 210 may be removed in small amounts, but this does not affect the gate structure 200 and the active region 100 located therebelow, so no additional mask may be required.

[0132] In this embodiment, when etching the sidewall material layer 231, an etchant with a relatively slow etching rate for the nitride dielectric layer 120 can be selected. Therefore, the nitride dielectric layer 120 is used as the etching stop layer of the sidewall material layer 231, so that the etching progress of the sidewall material layer 231 can be more accurately controlled, and the active area 100 at the bottom can be protected from being etched. When the etching of the sidewall material layer 231 is basically completed, the nitride dielectric layer 120 on the active area 100 is basically not etched. Then, the nitride dielectric layer 120 is removed. Since the etching rate difference between the nitride dielectric layer 120 and the active area 100 is large, and the removal amount when the nitride dielectric layer 120 is removed alone is easier to control, the active area 100 is significantly less damaged in the above steps.

[0133] It can be understood that the nitride dielectric layer 120 here is formed by the reaction of the oxidized dielectric layer 110. If the oxidized dielectric layer 110 is not reacted to form the nitride dielectric layer 120, that is, the oxidized dielectric layer 110 is still on the active area 100, then when the spacer material layer 231 is deposited, the oxidized dielectric layer 110 cannot effectively prevent the deposition material from reacting with the active area 100, resulting in oxidation damage to the active area 100. Furthermore, the etching progress of the spacer material layer 231 is more difficult to accurately control, and over-etching is prone to occur, resulting in over-etching damage to the active area 100.

[0134] Step S7, preparing source and drain regions in the active area not covered by the gate structure and the spacer structure.

[0135] Fig.11 Shown in Fig.10 The schematic diagram of the structure of preparing the source and drain regions 130 based on the structure shown in FIG. Fig.11 As shown, the source and drain regions 130 are located on a side of the spacer structure 230 away from the gate structure 200 .

[0136] In some examples of this embodiment, the source and drain regions 130 may be obtained by doping the active region 100 . It is understood that the doping concentration in the source and drain regions 130 should be higher than the doping concentration in the lightly doped drain region 140 .

[0137] In some examples of this embodiment, in the step of preparing the source and drain regions 130 , the active region 100 may be doped by ion implantation.

[0138] In some examples of this embodiment, after preparing the spacer structure 230 , the process further includes preparing a third protection layer covering the spacer structure 230 .

[0139] Fig.12 Shown in Fig.11 A schematic diagram of the structure of preparing the third protective layer 240 based on the structure shown in FIG. Fig.12 As shown, the third protection layer 240 covers the surface of the source and drain regions 130 , the surface of the spacer structure 230 , and the surface of the gate top protection layer 210 .

[0140] It can be understood that after the source and drain regions 130 are prepared, the third protection layer 240 can shield and protect the source and drain regions 130 and the sidewall structure 230 to facilitate the preparation of subsequent structures.

[0141] In some examples of this embodiment, the material of the third protective layer 240 may include one or more of silicon nitride, silicon oxide, and silicon oxynitride. In this embodiment, the material of the third protective layer 240 may include silicon nitride.

[0142] Step S8, preparing source-drain contacts on the source-drain region.

[0143] In some examples of this embodiment, the steps of preparing source-drain contacts include: forming an interlayer dielectric layer on a semiconductor substrate, forming a connection hole in the interlayer dielectric layer with the bottom exposing the source and drain regions; filling the connection hole with a conductive material electrically connected to the source and drain regions to form a source-drain contact.

[0144] In this embodiment, the interlayer dielectric layer may include a first interlayer dielectric layer and a second interlayer dielectric layer.

[0145] In some examples of this embodiment, the step of preparing source-drain contacts further includes preparing gate leads on the gate structure 200 .

[0146] The process of preparing source-drain contacts on the source-drain region 130 and preparing gate leads on the gate structure 200 can refer to Figure 13 to Figure 18 .

[0147] Fig.13 Shown in Fig.12 A schematic diagram of a structure in which a first interlayer dielectric layer 250, a second interlayer dielectric layer 260, a first pattern layer 320 and a second pattern layer 330 are sequentially stacked on the basis of the structure shown.

[0148] Reference Fig.13 As shown, the first interlayer dielectric layer 250 is disposed on the source / drain region 130 and the spacer structure 230 . In some examples of this embodiment, the first interlayer dielectric layer 250 has a flat surface, so that a flat second interlayer dielectric layer 260 can be prepared on the first interlayer dielectric layer 250 .

[0149] In some examples of this embodiment, a top end of the first interlayer dielectric layer 250 is flush with a top end of the third protection layer 240 .

[0150] In some examples of this embodiment, the material of the first interlayer dielectric layer 250 may include one or more of silicon nitride, silicon oxynitride, and silicon oxide. In this embodiment, the material of the first interlayer dielectric layer 250 is selected from silicon oxide.

[0151] Reference Fig.13 As shown, the second interlayer dielectric layer 260 is disposed on the first interlayer dielectric layer 250 and the third protection layer 240 .

[0152] In some examples of this embodiment, the material of the second interlayer dielectric layer 260 may include one or more of silicon nitride, silicon oxynitride, and silicon oxide. In this embodiment, the material of the second interlayer dielectric layer 260 is different from the material of the first interlayer dielectric layer 250, for example, the material of the second interlayer dielectric layer 260 is selected from silicon nitride.

[0153] Reference Fig.13 As shown, the first pattern layer 320 and the second pattern layer 330 are sequentially stacked on the second interlayer dielectric layer 260 .

[0154] In some examples of this embodiment, the materials of the first pattern layer 320 and the second pattern layer 330 may be different. For example, the material of the first pattern layer 320 may include a spin-on carbon hard mask material, and the material of the second pattern layer 330 may include one or more of silicon nitride, silicon oxide, and silicon oxynitride.

[0155] Fig.14 Shown in Fig.13 A schematic structural diagram of etching the second pattern layer 330, the first pattern layer 320, the second interlayer dielectric layer 260 and the first interlayer dielectric layer 250 based on the structure shown.

[0156] Reference Fig.14 As shown, the second pattern layer 330 is etched to form an opening defining the position of the connection hole. It is understood that before etching the second pattern layer 330, a photolithography layer can be prepared on the second pattern layer 330 to define the area to be etched of the second pattern layer 330. When etching the second pattern layer 330, the first pattern layer 320 can be used as an etching stop layer.

[0157] Reference Fig.14 As shown, it can be understood that the opening of the second pattern layer 330 is located on the source and drain region 130 .

[0158] Reference Fig.14As shown, the first pattern layer 320 is etched based on the second pattern layer 330 to transfer the pattern in the second pattern layer 330 to the first pattern layer 320. Therefore, the first pattern layer 320 has an opening corresponding to the second pattern layer 330. When etching the first pattern layer 320, the second interlayer dielectric layer 260 can be used as an etching stop layer.

[0159] Reference Fig.14 As shown, the second interlayer dielectric layer 260 is etched based on the first pattern layer 320 to transfer the pattern in the first pattern layer 320 to the second interlayer dielectric layer 260. Therefore, the second interlayer dielectric layer 260 has an opening corresponding to the first pattern layer 320. When etching the second interlayer dielectric layer 260, the first interlayer dielectric layer 250 can be used as an etching stop layer.

[0160] Reference Fig.14 As shown, the first interlayer dielectric layer 250 is etched based on the second interlayer dielectric layer 260 to transfer the pattern of the second interlayer dielectric layer 260 to the first interlayer dielectric layer 250 .

[0161] In addition, refer to Fig.14 As shown, when the first interlayer dielectric layer 250 is formed, the third protective layer 240 can be used as an etch stop layer, which requires that the material of the third protective layer 240 is different from the material of the first interlayer dielectric layer 250. By using the third protective layer 240 as the etch stop layer, the first interlayer dielectric layer 250 on the source and drain regions 130 can be removed to expose the third protective layer 240 on the source and drain regions 130.

[0162] Understandably, Fig.13 and Fig.14 The process shown is mainly used to form a connection hole in the interlayer dielectric layer, and the connection hole defines a subsequent preparation area for source and drain contacts.

[0163] Fig.15 Shown in Fig.14 Schematic diagram of the structure of preparing the third pattern layer 340 and the fourth pattern layer 350 based on the structure shown.

[0164] Reference Fig.15 As shown, the third pattern layer 340 is disposed on the third protection layer 240 and the second interlayer dielectric layer 260. In some examples of this embodiment, the third pattern layer 340 has a flat surface.

[0165] Reference Fig.15 As shown, the fourth pattern layer 350 is stacked on the third pattern layer 340 .

[0166] In some examples of this embodiment, the materials of the third pattern layer 340 and the fourth pattern layer 350 may be different. For example, the material of the third pattern layer 340 may include a spin-on carbon hard mask material, and the material of the fourth pattern layer 350 may include one or more of silicon nitride, silicon oxide, and silicon oxynitride. In addition, the material of the third pattern layer 340 and the second interlayer dielectric layer 260 and the material of the first interlayer dielectric layer 250 may all be different.

[0167] In some examples of this embodiment, the material of the third pattern layer 340 may be the same as the material of the first pattern layer 320. In the actual preparation process, the first pattern layer 320 that has been prepared may be retained, and the material of the third pattern layer 340 may be prepared on the basis of the first pattern layer 320 to form the third pattern material layer 340.

[0168] Fig.16 Shown in Fig.15 A schematic diagram of a structure in which a fourth pattern layer 350, a third pattern material layer 340, a second interlayer dielectric layer 260, a third protection layer 240 and a gate top protection layer 210 are etched on the basis of the structure shown.

[0169] Reference Fig.16 As shown, the fourth pattern layer 350 has an opening. It is understood that before etching the fourth pattern layer 350, a photoresist layer may be prepared on the fourth pattern layer 350 to define the area to be etched of the fourth pattern layer 350. When etching the fourth pattern layer 350, the third pattern layer 340 may be used as an etching stop layer.

[0170] Reference Fig.16 As shown, it can be understood that the opening in the fourth pattern layer 350 is located on the gate structure 200 .

[0171] Reference Fig.16 As shown, the third pattern layer 340 is etched based on the fourth pattern layer 350 to transfer the pattern in the fourth pattern layer 350 to the third pattern layer 340. Therefore, the third pattern layer 340 has an opening corresponding to the fourth pattern layer 350. When etching the third pattern layer 340, the second interlayer dielectric layer 260 can be used as an etching stop layer.

[0172] Reference Fig.16 As shown, the second interlayer dielectric layer 260 is further etched based on the third pattern layer 340. The pattern in the third pattern layer 340 is also transferred to the second interlayer dielectric layer 260. Therefore, the second interlayer dielectric layer 260 also has an opening corresponding to the third pattern layer 340.

[0173] Reference Fig.16As shown, the third protection layer 240 and the gate top protection layer 210 are etched based on the third pattern layer 340. The pattern in the third pattern layer 340 is also transferred to the third protection layer 240 and the gate top protection layer 210, so the third protection layer 240 and the gate top protection layer 210 also have openings connected to the third pattern layer 340.

[0174] In some examples of this embodiment, when etching the gate top protection layer 210 , the etching amount may be controlled so as not to etch through the gate top protection layer 210 , so as to temporarily protect the second gate conductive layer 203 .

[0175] Fig.17 Shown in Fig.16 Schematic diagram of a structure in which the third pattern layer 340 and the fourth pattern layer 350 are removed from the structure shown in FIG. Further, after removing the third pattern layer 340 and the fourth pattern layer 350, the steps of removing the remaining portion of the gate top protection layer 210 on the second gate conductive layer 203 and removing the remaining third protection layer 240 on the source and drain regions 130 are also included to expose the second gate conductive layer 203 and the source and drain regions 130, respectively.

[0176] in, Figure 15 to Figure 17 The process shown is for forming a gate lead hole exposing the gate structure 200 .

[0177] Reference Fig.17 As shown, after removing the third pattern layer 340 and the fourth pattern layer 350, the gate top protection layer 210 on the gate structure 200 is etched to expose the gate structure 200. The third protection layer 240 on the source and drain regions 130 is etched to expose the source and drain regions 130. The remaining portion of the third protection layer 240 can be used to protect the sidewall structure 230.

[0178] In some examples of this embodiment, the material of the third protection layer 240 is the same as that of the gate top protection layer 210. Therefore, the gate top protection layer 210 and the third protection layer 240 can be etched in the same etching process.

[0179] Fig.18 Shown in Fig.17 A schematic diagram of a structure for preparing source-drain contacts 410 and gate leads 420 based on the structure shown. Fig.18 As shown, the source-drain contact 410 is electrically connected to the source-drain region 130. Further, the source-drain contact 410 directly contacts the source-drain region 130. The gate lead 420 is electrically connected to the gate structure 200. Further, the gate lead 420 directly contacts the gate structure 200.

[0180] Reference Fig.18As shown, the source-drain contact 410 and the gate lead 420 may be separated by a first interlayer dielectric layer 250 and a second interlayer dielectric layer 260 .

[0181] In some examples of this embodiment, the step of preparing the source-drain contact 410 and the gate lead 420 may include: depositing a conductive material on the source-drain region 130 and the gate structure 200, and then etching back the conductive material to form the source-drain contact 410 and the gate lead 420 with insulation spacing, respectively. The conductive material may be a metal material, such as one or more of copper, aluminum, gold, silver and tungsten. In this embodiment, the conductive material is tungsten.

[0182] Understandably, through Figure 13 to Figure 18 The described preparation method can complete the preparation of the source-drain contacts 410 and the gate leads 420 .

[0183] Through steps S1 to S8, the preparation of the semiconductor structure provided by the present disclosure can be completed.

[0184] Furthermore, the present disclosure also provides a Fig.18 The semiconductor structure shown includes an active region 100, a gate structure 200, a spacer structure 230 and a nitride dielectric layer 120. The active region 100 is provided with a lightly doped drain region 140 and a source / drain region 130, the gate structure 200 is provided on the active region 100, the spacer structure 230 is provided on the sidewall of the gate structure 200, and the nitride dielectric layer 120 is provided between the spacer structure 230 and the active region 100.

[0185] Compared with the traditional semiconductor structure, the nitride dielectric layer 120 is introduced into the manufacturing process of the semiconductor structure, which can better protect the active area 100 and reduce the oxidation damage and over-etching damage of the source and drain area 130 during the manufacturing process, thereby improving the stability of the semiconductor device.

[0186] Further, refer to Fig.18 As shown, the semiconductor structure may further include source-drain contacts 410 and gate leads 420 . The source-drain contacts 410 are disposed on and in contact with the source-drain regions 130 , and the gate leads 420 are disposed on and in contact with the gate structure 200 .

[0187] Please note that the above embodiments are for illustrative purposes only and are not meant to limit the present disclosure.

[0188] It should be understood that, unless otherwise specified herein, the execution of the steps described is not strictly limited in order, and the steps may be executed in other orders. Moreover, at least a portion of the steps described may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.

[0189] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0190] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. A method for preparing a semiconductor structure, characterized in that: The steps include: Providing a semiconductor substrate, the semiconductor substrate comprising an active region; forming a gate structure on the active area; Performing nitridation treatment on the active area not covered by the gate structure to form a nitrided dielectric layer, and then preparing a lightly doped drain region in the active area under the nitrided dielectric layer; forming a sidewall structure on the sidewall of the gate structure; A source and drain region is prepared in the active region not covered by the gate structure and the spacer structure.

2. The method for preparing a semiconductor structure according to claim 1, characterized in that: Before the nitridation treatment is performed, the surface of the active area not covered by the gate structure has an oxide dielectric layer; During the nitridation treatment, the oxidized dielectric layer is transformed into the nitrided dielectric layer.

3. The method for preparing a semiconductor structure according to claim 2, characterized in that: The nitridation treatment includes: using a reaction gas to transform the oxidized dielectric layer into the nitrided dielectric layer in a remote plasma nitridation treatment manner, wherein the reaction gas includes a nitrogen source gas and a reducing gas.

4. The method for preparing a semiconductor structure according to claim 3, characterized in that: In the reaction gas, the flow ratio of the nitrogen source gas to the reducing gas is 1:0.5 to 1:3; and / or, During the nitridation treatment, the reaction temperature is controlled to be 30° C. to 60° C.; and / or, During the nitriding process, the reaction time is controlled to be 30s to 180s.

5. The method for preparing a semiconductor structure according to claim 2, characterized in that: During the nitridation treatment, the thickness of the formed nitrided dielectric layer is controlled to be 5 nm to 30 nm.

6. The method for preparing a semiconductor structure according to any one of claims 2 to 5, characterized in that: After forming the gate structure and before performing the nitridation treatment, the method further includes: forming a first protective layer, wherein the first protective layer covers a surface of the gate structure and a surface of the active area not covered by the gate structure; forming a second protective layer, wherein the second protective layer covers the surface of the first protective layer; Etching the second protection layer and the first protection layer covering the surface of the active area to expose the active area not covered by the gate structure; and, The second protection layer on the sidewall of the gate structure is removed and at least the first protection layer covering the sidewall of the gate structure is retained.

7. The method for preparing a semiconductor structure according to claim 6, characterized in that: The material of the first protective layer is different from the material of the oxidizing medium layer, and the material of the first protective layer includes nitride; and / or, The material of the second protection layer is different from that of the first protection layer, and the material of the second protection layer includes oxide.

8. The method for preparing a semiconductor structure according to claim 7, characterized in that: Forming a spacer structure on the sidewall of the gate structure includes: forming a spacer material layer, wherein the spacer material layer covers the surface of the first protective layer and the nitride dielectric layer; The sidewall material layer on the nitride dielectric layer is etched using the nitride dielectric layer as an etch stop layer, and a portion of the sidewall material layer on both sides of the gate structure is retained to serve as the sidewall structure.

9. The method for preparing a semiconductor structure according to any one of claims 1 to 5 and 7 to 8, characterized in that: After the source and drain regions are prepared, the method further includes the step of preparing source and drain contacts on the source and drain regions. The step of preparing the source and drain contacts includes: forming an interlayer dielectric layer on the semiconductor substrate, and forming a connection hole in the interlayer dielectric layer with the bottom exposing the source and drain regions; The connection hole is filled with a conductive material electrically connected to the source and drain regions to form the source and drain contacts.

10. A semiconductor structure, characterized in that: include: A semiconductor substrate, wherein an active region is provided in the semiconductor substrate, and wherein a lightly doped drain region and a source-drain region are provided in the active region; A gate structure, wherein the gate structure is disposed on the active region, and the lightly doped drain region and the source-drain region are not covered by the gate structure; A sidewall structure, wherein the sidewall structure is disposed on a sidewall of the gate structure; A nitride dielectric layer, wherein the nitride dielectric layer is not covered by the gate structure, the nitride dielectric layer is arranged between the sidewall structure and the active area, the lightly doped drain area is arranged under the nitride dielectric layer and covered by the nitride dielectric layer, and the source and drain areas are arranged on a side of the nitride dielectric layer away from the gate structure.

Citation Information

Patent Citations

  • Method for manufacturing MOS transistor

    CN102044434A

  • Semiconductor device and manufacture method thereof

    CN102347226A

  • Method for forming auxiliary side wall

    CN102487003A

  • Semiconductor structure forming method and transistor

    CN112652578A

  • Manufacturing method of semiconductor device

    CN115020343A