Organic photovoltaic cell with magnetic GO-doped hole transport layer and preparation method of organic photovoltaic cell
By using magnetic GO-doped PEDOT:PSS as the hole transport layer material in organic photovoltaic cells, the stability problems caused by high hygroscopicity and acidity of PEDOT:PSS are solved, and the conductivity and stability are improved, and the photoelectric conversion is improved. Efficiency and short circuit current density.
Patent Information
- Application Number
- CN202410999576.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
AI Technical Summary
The high hygroscopicity and acidity of the hole transport layer material PEDOT:PSS in existing organic photovoltaic cells lead to a decrease in the long-term stability of the device, and its low conductivity leads to an increase in the transfer resistance at the device interface, affecting the photoelectric conversion efficiency.
Using magnetic GO doped PEDOT:PSS as the hole transport layer material, the conductivity and stability of the hole transport layer are improved by mixing Fe3O4/GO magnetic nanocomposite material and PEDOT:PSS, and spin coating process and annealing. The process forms an organic photovoltaic cell structure.
It significantly reduces the chance of charge recombination at the interface, improves hole mobility, improves the short-circuit current density and filling factor of organic photovoltaic cells, achieves high photoelectric conversion efficiency, and improves the overall stability of the device.
Smart Images

Figure CN118900575A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of organic solar cells, and in particular relates to an organic photovoltaic cell with a magnetic GO-doped hole transport layer and a preparation method thereof. Background Art
[0002] Organic photovoltaic cells have become one of the fastest-growing and most dynamic new energy research hotspots in recent years due to their flexibility, lightweight and roll-to-roll processing potential. Currently, the photoelectric conversion efficiency of single-junction organic photovoltaic cells (OSCs) has exceeded 19%, while the photoelectric conversion efficiency of tandem devices has reached 20%. This remarkable progress is mainly due to the rapid development of non-fullerene acceptors and polymer donors, as well as a deep understanding of device and interface engineering.
[0003] In organic photovoltaic cells, the ideal hole transport layer material should have the advantages of high transparency, matching of energy levels with the active layer, and excellent electrical properties. At present, the hole transport layer material is mainly PEDOT:PSS. However, due to the high hygroscopicity and acidity of PEDOT:PSS, the long-term stability of the device is reduced. There are many solutions to the above problems, including the modification of PEDOT:PSS and the development of other materials to replace PEDOT:PSS as the hole transport layer.
[0004] Graphene oxide (GO) has become a potential hole transport layer material due to its solution processability, unique two-dimensional structure, and tunable electronic properties caused by functionalization. GO not only has a high work function, but also exhibits superior performance. However, its low conductivity leads to significantly increased transfer resistance at the device interface. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides an organic photovoltaic cell with a magnetic GO-doped hole transport layer and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0006] The present invention provides an organic photovoltaic cell with a magnetic GO-doped hole transport layer, comprising: an ITO anode, a hole transport layer, an active layer, an electron transport layer and a metal cathode arranged in sequence from bottom to top, wherein the material of the hole transport layer is magnetic GO-doped PEDOT:PSS.
[0007] In one embodiment of the present invention, the thickness of the hole transport layer is 20-30 nm.
[0008] In one embodiment of the present invention, the magnetic GO is a Fe3O4 / GO magnetic nanocomposite material.
[0009] In one embodiment of the present invention, the material of the active layer is PM6:L8-BO, and the thickness is 90-110 nm.
[0010] In one embodiment of the present invention, the material of the electron transport layer is PNDIT-F3N, and the thickness is 5-10 nm.
[0011] The present invention provides a method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer, which is applicable to the organic photovoltaic cell with a magnetic GO-doped hole transport layer described in any one of the above embodiments, and the preparation method comprises:
[0012] Step 1: Surface pretreatment of ITO glass;
[0013] Step 2: preparing a hole transport layer spin coating liquid, spin coating the hole transport layer spin coating liquid on the ITO glass after surface pretreatment by spin coating process, and then annealing to obtain a hole transport layer; wherein the material of the hole transport layer is magnetic GO-doped PEDOT:PSS;
[0014] Step 3: preparing an active layer spin coating liquid, spin coating the active layer spin coating liquid on the hole transport layer by a spin coating process, and then performing annealing treatment to obtain an active layer;
[0015] Step 4: preparing an electron transport layer spin coating liquid, and spin coating the electron transport layer spin coating liquid on the active layer by a spin coating process to obtain an electron transport layer;
[0016] Step 5: Prepare a metal cathode on the electron transport layer by using an evaporation process.
[0017] In one embodiment of the present invention, step 1 comprises:
[0018] Step 1.1: ultrasonically clean the ITO glass with deionized water, acetone, detergent, deionized water and isopropanol in sequence;
[0019] Step 1.2: Drying the ITO glass after ultrasonic cleaning;
[0020] Step 1.3: The dried ITO glass surface is treated with ozone plasma.
[0021] In one embodiment of the present invention, step 2 comprises:
[0022] Step 2.1: Disperse the prepared Fe3O4 nanoparticles in an ethanol solution, add GO nanosheets to the mixed solution of Fe3O4 nanoparticles and ethanol, and load the Fe3O4 nanoparticles on the GO surface by stirring to form magnetic GO;
[0023] Step 2.2: Dispersing magnetic GO in deionized water to obtain a magnetic GO aqueous solution with a concentration of 0.01-0.1 mg / ml;
[0024] Step 2.3: Mixing the magnetic GO aqueous solution and PEDOT:PSS in a volume ratio of 1:1 to obtain the hole transport layer spin coating solution;
[0025] Step 2.4: Spin coating the hole transport layer spin coating liquid onto the surface pretreated ITO glass using a spin coating process, and then perform annealing to obtain the hole transport layer, wherein the annealing temperature is 120-150° C. and the time is 10-20 min.
[0026] In one embodiment of the present invention, step 3 comprises:
[0027] Step 3.1: PM6 and L8-BO in a mass ratio of 1:1.2 are dissolved in chloroform containing 0.3% DIO as an additive, and stirred at room temperature for 12 hours to obtain the active layer spin coating solution, wherein the total concentration of PM6 and L8-BO in the active layer spin coating solution is 13.2-16.5 mg / ml;
[0028] Step 3.2: Spin-coat the active layer spin-coating liquid on the hole transport layer using a spin-coating process, and then perform annealing to obtain the active layer, wherein the annealing temperature is 90-120° C. and the time is 10-15 min.
[0029] In one embodiment of the present invention, step 4 comprises:
[0030] Step 4.1: dissolving PNDIT-F3N in methanol containing 0.5% glacial acetic acid to obtain the electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution is 0.5-1 mg / ml;
[0031] Step 4.2: Spin-coating the electron transport layer spin-coating liquid on the active layer using a spin-coating process to obtain the electron transport layer.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The organic photovoltaic cell with a magnetic GO-doped hole transport layer of the present invention uses magnetic GO-doped PEDOT:PSS as the hole transport layer of the organic photovoltaic cell, and the hole transport layer has an energy level matching the active layer and a high conductivity. The addition of magnetic GO significantly reduces the probability of charge recombination at the interface, improves the hole mobility, thereby improving the short-circuit current density and fill factor of the organic photovoltaic cell, and finally achieves a high photoelectric conversion efficiency of the organic photovoltaic cell; in addition, compared with the device with PEDOT:PSS as the hole transport layer, the addition of inorganic materials reduces the problem of device stability degradation caused by the high humidity and acidity of PEDOT:PSS to a certain extent, thereby improving the overall stability of the device.
[0034] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic structural diagram of an organic photovoltaic cell with a magnetic GO-doped hole transport layer provided in an embodiment of the present invention;
[0036] Figure 2 is an XRD diagram of a Fe3O4 / GO magnetic nanocomposite material provided in an embodiment of the present invention;
[0037] Figure 3 It is a flow chart of a method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the following is a detailed description of an organic photovoltaic cell with a magnetic GO-doped hole transport layer and a preparation method thereof proposed in accordance with the present invention in combination with the accompanying drawings and specific implementation methods.
[0039] The above and other technical contents, features and effects of the present invention are clearly presented in the following detailed description of the specific implementation modes in conjunction with the accompanying drawings. Through the description of the specific implementation modes, the technical means and effects adopted by the present invention to achieve the predetermined purpose can be more deeply and specifically understood. However, the attached drawings are only for reference and explanation purposes and are not used to limit the technical solutions of the present invention.
[0040] In the first aspect, the present invention provides an organic photovoltaic cell with a magnetic GO doped hole transport layer, see Figure 1 , Figure 1Schematic diagram of the structure of an organic photovoltaic cell with a hole transport layer doped with magnetic GO provided in an embodiment of the present invention. Figure 1 As shown, the organic photovoltaic cell with a magnetic GO-doped hole transport layer of this embodiment includes: an ITO anode 01, a hole transport layer 02, an active layer 03, an electron transport layer 04 and a metal cathode 05 arranged in sequence from bottom to top.
[0041] In an optional embodiment of the present invention, the ITO anode is indium tin oxide glass.
[0042] In this embodiment, the material of the hole transport layer is magnetic GO doped PEDOT:PSS with a thickness of 20-30 nm. The magnetic GO is a Fe3O4 / GO magnetic nanocomposite material. Among them, PEDOT:PSS is composed of two substances, PEDOT and PSS, PEDOT is a polymer of EDOT (3,4-ethylenedioxythiophene monomer), and PSS is polystyrene sulfonate.
[0043] In an optional embodiment of the present invention, the material of the active layer is PM6:L8-BO, and the thickness is 90-110 nm.
[0044] In an optional embodiment of the present invention, the material of the electron transport layer is PNDIT-F3N, and the thickness is 5-10 nm.
[0045] In an optional embodiment of the present invention, the metal cathode is a silver electrode with a thickness of 150 nm.
[0046] In this embodiment, since the PEDOT:PSS doped with magnetic GO has good light transmittance, the work function and conductivity of the hole transport layer are improved, so that the hole transport layer has an energy level matching that of the active layer. Secondly, magnetic GO doping can improve the surface morphology rearrangement of the hole transport layer and reduce the interface energy barrier. Introducing magnetic GO doped PEDOT:PSS as a mixed hole transport layer into PM6:L8-BO-based OSCs can enhance the ohmic contact between the electrode and the active layer, improve the charge transfer and collection efficiency, reduce the recombination process, and improve the hole mobility, thereby improving the short-circuit current density and fill factor of the organic photovoltaic cell, and finally achieving a high photoelectric conversion efficiency of the organic photovoltaic cell.
[0047] The organic photovoltaic cell with a magnetic GO-doped hole transport layer in the embodiment of the present invention uses magnetic GO-doped PEDOT:PSS as the hole transport layer of the organic photovoltaic cell, and the hole transport layer has an energy level matching the active layer and a higher conductivity. The addition of magnetic GO significantly reduces the probability of charge recombination at the interface between the hole transport layer and the active layer, improves the hole mobility, thereby improving the short-circuit current density and fill factor of the organic photovoltaic cell, and ultimately achieves a high photoelectric conversion efficiency of the organic photovoltaic cell. In addition, compared with the device with PEDOT:PSS as the hole transport layer, the addition of inorganic materials reduces the problem of decreased device stability caused by the high humidity and acidity of PEDOT:PSS to a certain extent, thereby improving the overall stability of the device. This is because the addition of inorganic materials can adjust the work function of PEDOT:PSS, which helps to optimize the energy level arrangement of the device, thereby improving the efficiency and stability of the device. Secondly, inorganic materials usually have higher chemical stability and lower hygroscopicity, and are not easy to react with substances such as water. PEDOT:PSS is highly hydrophilic and acidic, which will cause it to corrode the ITO anode and cause indium to diffuse into the active layer, thereby reducing the stability of the device. When inorganic materials are added to PEDOT:PSS, the hygroscopicity and acidity of the entire composite material can be reduced, thereby improving the stability of the device. Furthermore, the addition of inorganic materials is beneficial to improving the electrical properties of PEDOT:PSS, thereby reducing defects at the interface and improving the overall stability of the device.
[0048] In a second aspect, an embodiment of the present invention provides a method for preparing an organic photovoltaic cell having a magnetic GO-doped hole transport layer, which is applicable to the organic photovoltaic cell having a magnetic GO-doped hole transport layer provided in the first aspect.
[0049] See also Figure 3 , Figure 3 is a flow chart of a method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer provided in an embodiment of the present invention, such as Figure 3 As shown, the preparation method of the organic photovoltaic cell with a magnetic GO-doped hole transport layer of this embodiment includes:
[0050] Step 1: Surface pretreatment of ITO glass.
[0051] In an optional embodiment, step 1 includes:
[0052] Step 1.1: Ultrasonic cleaning of ITO glass was performed with deionized water, acetone, detergent, deionized water and isopropanol in sequence.
[0053] Optionally, the ITO glass may be ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol in sequence for 15 minutes each.
[0054] Step 1.2: Dry the ITO glass after ultrasonic cleaning.
[0055] Optionally, the ITO glass after ultrasonic cleaning can be dried in an oven or blown dry with nitrogen.
[0056] Step 1.3: The dried ITO glass surface is treated with ozone plasma.
[0057] Optionally, the ITO glass surface after the drying treatment may be subjected to ozone plasma treatment for 20 minutes.
[0058] Step 2: prepare a hole transport layer spin coating liquid, spin-coat the hole transport layer spin coating liquid on the ITO glass after surface pretreatment by spin coating process, and then perform annealing treatment to obtain the hole transport layer.
[0059] Among them, the material of the hole transport layer is magnetic GO-doped PEDOT:PSS.
[0060] In an optional embodiment, step 2 includes:
[0061] Step 2.1: The prepared Fe3O4 nanoparticles are dispersed in an ethanol solution, GO nanosheets are added to the mixed solution of Fe3O4 nanoparticles and ethanol, and the Fe3O4 nanoparticles are loaded on the GO surface by stirring to form magnetic GO.
[0062] Alternatively, Fe3O4 nanoparticles can be prepared by solvothermal method.
[0063] In this embodiment, GO nanosheets were added to a mixed solution of Fe3O4 nanoparticles and ethanol and stirred for 1 hour to load the Fe3O4 nanoparticles on the surface of GO and co-precipitate to form a Fe3O4 / GO magnetic nanocomposite material, namely magnetic GO.
[0064] It should be noted that in the process of preparing magnetic GO, there is no limit on the ratio of Fe3O4 nanoparticles to GO nanosheets, and more Fe3O4 nanoparticles can be added. After the magnetic GO is prepared, the Fe3O4 nanoparticles not loaded on GO are washed away with anhydrous ethanol and water.
[0065] See also Figure 2 , Figure 2 This is an XRD diagram of a Fe3O4 / GO magnetic nanocomposite material provided in an embodiment of the present invention. It can be seen from the figure that the Fe3O4 / GO magnetic nanocomposite material is successfully prepared.
[0066] Step 2.2: Disperse magnetic GO in deionized water to obtain a magnetic GO aqueous solution with a concentration of 0.01-0.1 mg / ml.
[0067] In this embodiment, after the magnetic GO is dispersed in the deionized water, it can be subjected to ultrasonic treatment for 2 hours to make the magnetic GO uniformly dispersed in the deionized water.
[0068] Step 2.3: Mix the magnetic GO aqueous solution and PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0069] Step 2.4: Spin coating the hole transport layer spin coating liquid onto the surface pretreated ITO glass using a spin coating process, and then perform annealing to obtain the hole transport layer, wherein the annealing temperature is 120-150° C. and the time is 10-20 min.
[0070] Optionally, the rotation speed of spin coating the hole transport layer spin coating liquid is 4500 rpm, and the spin coating time is 20 s.
[0071] Step 3: prepare an active layer spin coating liquid, spin-coat the active layer spin coating liquid on the hole transport layer using a spin coating process, and then perform annealing to obtain the active layer.
[0072] In an optional embodiment, step 3 includes:
[0073] Step 3.1: PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.2-16.5 mg / ml.
[0074] Step 3.2: Spin coating the active layer spin coating liquid onto the hole transport layer using a spin coating process, and then perform annealing to obtain the active layer, wherein the annealing temperature is 90-120° C. and the time is 10-15 min.
[0075] Optionally, the rotation speed of the spin coating liquid for spin coating the active layer is 3000 rpm, and the spin coating time is 20 s.
[0076] Step 4: prepare an electron transport layer spin coating liquid, and spin-coat the electron transport layer spin coating liquid on the active layer using a spin coating process to obtain an electron transport layer.
[0077] In an optional embodiment, step 4 includes:
[0078] Step 4.1: PNDIT-F3N is dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution is 0.5-1 mg / ml.
[0079] Step 4.2: Spin-coat the electron transport layer spin-coating liquid on the active layer using a spin-coating process to obtain an electron transport layer.
[0080] Optionally, the rotation speed of spin coating the electron transport layer spin coating liquid is 3000 rpm, and the spin coating time is 20 s.
[0081] Step 5: Prepare a metal cathode on the electron transport layer using an evaporation process.
[0082] Alternatively, a vacuum coating apparatus may be used to coat metal Ag with The rate of evaporation is 4×10 -4 The thickness of the metal cathode can be 150 nm.
[0083] Furthermore, the effects of the organic photovoltaic cell with a magnetic GO-doped hole transport layer and the preparation method thereof of the present invention are described through specific examples and comparative examples.
[0084] Example 1
[0085] An organic photovoltaic cell with magnetic GO doped with PEDOT:PSS as a hole transport layer was prepared with a doping amount of magnetic GO of 1%wt. The structure of the organic photovoltaic cell from bottom to top is: ITO anode / magnetic GO:PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method is as follows:
[0086] Step (1): ITO glass surface pretreatment.
[0087] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0088] Step (2): Prepare a magnetic GO-doped PEDOT:PSS hole transport layer.
[0089] Fe3O4 nanoparticles were prepared by solvothermal method. The Fe3O4 nanoparticles were dispersed in ethanol solution. GO nanosheets were added to the mixed solution of Fe3O4 nanoparticles and ethanol and stirred for 1 h to load the Fe3O4 nanoparticles on the GO surface. Fe3O4 / GO magnetic nanocomposite materials were co-precipitated as magnetic GO.
[0090] Magnetic GO was dispersed in deionized water and ultrasonicated for 2 h to obtain a magnetic GO aqueous solution with a concentration of 0.01 mg / ml. The magnetic GO aqueous solution was mixed with PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0091] The hole transport layer spin coating liquid was spin coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0092] Step (3): Prepare PM6:L8-BO active layer.
[0093] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0094] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0095] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0096] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0097] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0098] Step (5): Prepare a metal cathode.
[0099] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0100] Example 2
[0101] An organic photovoltaic cell with magnetic GO doped with PEDOT:PSS as a hole transport layer was prepared with a doping amount of magnetic GO of 5%wt. The structure of the organic photovoltaic cell from bottom to top is: ITO anode / magnetic GO:PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method is as follows:
[0102] Step (1): ITO glass surface pretreatment.
[0103] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0104] Step (2): Prepare a magnetic GO-doped PEDOT:PSS hole transport layer.
[0105] Fe3O4 nanoparticles were prepared by solvothermal method. The Fe3O4 nanoparticles were dispersed in ethanol solution. GO nanosheets were added to the mixed solution of Fe3O4 nanoparticles and ethanol and stirred for 1 h to load the Fe3O4 nanoparticles on the GO surface. Fe3O4 / GO magnetic nanocomposite materials were co-precipitated as magnetic GO.
[0106] Magnetic GO was dispersed in deionized water and ultrasonicated for 2 h to obtain a magnetic GO aqueous solution with a concentration of 0.05 mg / ml. The magnetic GO aqueous solution was mixed with PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0107] The hole transport layer spin coating liquid was spin coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0108] Step (3): Prepare PM6:L8-BO active layer.
[0109] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0110] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0111] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0112] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0113] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0114] Step (5): Prepare a metal cathode.
[0115] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0116] Example 3
[0117] An organic photovoltaic cell with magnetic GO doped with PEDOT:PSS as a hole transport layer was prepared with a doping amount of magnetic GO of 10%wt. The structure of the organic photovoltaic cell from bottom to top is: ITO anode / magnetic GO:PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method is as follows:
[0118] Step (1): ITO glass surface pretreatment.
[0119] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0120] Step (2): Prepare a magnetic GO-doped PEDOT:PSS hole transport layer.
[0121] Fe3O4 nanoparticles were prepared by solvothermal method. The Fe3O4 nanoparticles were dispersed in ethanol solution. GO nanosheets were added to the mixed solution of Fe3O4 nanoparticles and ethanol and stirred for 1 h to load the Fe3O4 nanoparticles on the GO surface. Fe3O4 / GO magnetic nanocomposite materials were co-precipitated as magnetic GO.
[0122] Magnetic GO was dispersed in deionized water and ultrasonicated for 2 h to obtain a magnetic GO aqueous solution with a concentration of 0.1 mg / ml. The magnetic GO aqueous solution was mixed with PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0123] The hole transport layer spin coating liquid was spin coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0124] Step (3): Prepare PM6:L8-BO active layer.
[0125] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0126] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0127] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0128] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0129] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0130] Step (5): Prepare a metal cathode.
[0131] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0132] Comparative Example 1
[0133] An organic photovoltaic cell with PEDOT:PSS as a hole transport layer was prepared. The structure of the organic photovoltaic cell from bottom to top was: ITO anode / PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method was as follows:
[0134] Step (1): ITO glass surface pretreatment.
[0135] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0136] Step (2): Prepare a PEDOT:PSS hole transport layer.
[0137] The PEDOT:PSS solution was spin-coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0138] Step (3): Prepare PM6:L8-BO active layer.
[0139] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0140] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0141] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0142] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0143] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0144] Step (5): Prepare a metal cathode.
[0145] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0146] Comparative Example 2
[0147] An organic photovoltaic cell with GO-doped PEDOT:PSS as a hole transport layer was prepared with a GO doping amount of 1%wt. The structure of the organic photovoltaic cell from bottom to top is: ITO anode / GO:PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method is as follows:
[0148] Step (1): ITO glass surface pretreatment.
[0149] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0150] Step (2): Prepare a GO-doped PEDOT:PSS hole transport layer.
[0151] GO nanosheets were dispersed in deionized water and ultrasonicated for 2 h to obtain a GO aqueous solution with a concentration of 0.01 mg / ml. The GO aqueous solution was mixed with PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0152] The hole transport layer spin coating liquid was spin coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0153] Step (3): Prepare PM6:L8-BO active layer.
[0154] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0155] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0156] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0157] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0158] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0159] Step (5): Prepare a metal cathode.
[0160] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0161] Comparative Example 3
[0162] An organic photovoltaic cell with GO-doped PEDOT:PSS as a hole transport layer was prepared with a GO doping amount of 5%wt. The structure of the organic photovoltaic cell from bottom to top is: ITO anode / GO:PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method is as follows:
[0163] Step (1): ITO glass surface pretreatment.
[0164] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0165] Step (2): Prepare a GO-doped PEDOT:PSS hole transport layer.
[0166] GO nanosheets were dispersed in deionized water and ultrasonicated for 2 h to obtain a GO aqueous solution with a concentration of 0.05 mg / ml. The GO aqueous solution was mixed with PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0167] The hole transport layer spin coating liquid was spin coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0168] Step (3): Prepare PM6:L8-BO active layer.
[0169] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0170] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0171] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0172] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0173] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0174] Step (5): Prepare a metal cathode.
[0175] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0176] Comparative Example 4
[0177] An organic photovoltaic cell with GO-doped PEDOT:PSS as a hole transport layer was prepared with a GO doping amount of 10% wt. The structure of the organic photovoltaic cell from bottom to top is: ITO anode / GO:PEDOT:PSS / PM6:L8-BO / PNDIT-F3N / Ag. The specific preparation method is as follows:
[0178] Step (1): ITO glass surface pretreatment.
[0179] The ITO glass was ultrasonically cleaned with deionized water, acetone, detergent, deionized water and isopropanol for 15 minutes each, and the ITO glass after ultrasonic cleaning was dried in an oven or blown dry with nitrogen. The surface of the dried ITO glass was treated with ozone plasma for 20 minutes.
[0180] Step (2): Prepare a GO-doped PEDOT:PSS hole transport layer.
[0181] GO nanosheets were dispersed in deionized water and ultrasonicated for 2 h to obtain a GO aqueous solution with a concentration of 0.1 mg / ml. The GO aqueous solution was mixed with PEDOT:PSS in a volume ratio of 1:1 to obtain a hole transport layer spin coating solution.
[0182] The hole transport layer spin coating liquid was spin coated on the surface pretreated ITO glass by spin coating process, wherein the rotation speed was 4500 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain a hole transport layer with a thickness of 20 nm, wherein the annealing temperature was 150° C. and the time was 15 min.
[0183] Step (3): Prepare PM6:L8-BO active layer.
[0184] PM6 and L8-BO in a mass ratio of 1:1.2 were dissolved in chloroform with an additive of 0.3% DIO, and stirred at room temperature for 12 hours to obtain an active layer spin coating solution. The total concentration of PM6 and L8-BO in the active layer spin coating solution was 13.5 mg / ml.
[0185] The active layer spin coating liquid was spin coated on the hole transport layer by spin coating process, wherein the rotation speed was 3000 rpm and the spin coating time was 20 s, and then annealing treatment was performed to obtain an active layer with a thickness of 100 nm, wherein the annealing temperature was 90° C. and the time was 10 min.
[0186] Step (4): Prepare a PNDIT-F3N electron transport layer.
[0187] PNDIT-F3N was dissolved in methanol containing 0.5% glacial acetic acid to obtain an electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution was 1 mg / ml.
[0188] The electron transport layer spin coating liquid was spin coated on the active layer by spin coating process, the rotation speed was 3000 rpm, the spin coating time was 20 s, and the electron transport layer with a thickness of 10 nm was obtained.
[0189] Step (5): Prepare a metal cathode.
[0190] The metal Ag was coated by vacuum coating equipment. The metal cathode is deposited onto the electron transport layer at a rate of 100 nm to form a metal cathode with a thickness of 150 nm. The vacuum degree during the deposition process is 4×10 -4 Pause and proceed.
[0191] The performance parameters of the organic photovoltaic cells of Examples 1-3 and Comparative Examples 1-4 were measured. The measurement results are shown in Table 1.
[0192] Table 1 Performance parameters of organic photovoltaic cells of the embodiments and comparative examples
[0193]
[0194]
[0195] As can be seen from Table 1, the energy conversion efficiencies of the organic photovoltaic cells doped with 1wt%, 5wt% and 10wt% GO are 18.30%, 18.69% and 18.33%, respectively, while the energy conversion efficiencies of the organic photovoltaic cells doped with 1wt%, 5wt% and 10wt% magnetic GO are 18.49%, 18.91% and 18.29%, respectively. Among them, the organic photovoltaic cell with a doping ratio of 5wt% magnetic GO showed the highest photoelectric conversion efficiency, with an energy conversion efficiency of 18.91%, an open circuit voltage of 0.884V, and a short circuit current density of 26.93mA cm -2 And the filling factor is 79.45%. It is not difficult to find that the photoelectric conversion efficiency of PEDOT:PSS is greatly improved by adding magnetic GO.
[0196] As can be seen from Table 1, after doping magnetic GO in PEDOT:PSS, the photoelectric conversion efficiency of organic photovoltaic cells is significantly improved. PEDOT:PSS with an appropriate amount of magnetic GO doped magnetic nanocomposites has good transmittance, improved work function and conductivity, improved surface morphology rearrangement, and reduced interface energy barriers. The introduction of magnetic GO-doped PEDOT:PSS as a hybrid hole transport layer into PM6:L8-BO-based OSCs enhances the ohmic contact between the electrode and the active layer, improves the charge transfer and collection efficiency, and reduces the recombination process. At the same time, the stability of the hybrid HTL device is improved. This enhancement effect has also been verified in devices with other active layer systems, highlighting the effectiveness and universality of the method proposed in this invention. Therefore, magnetic GO-doped PEDOT:PSS will become a promising candidate for hole transport layers in high-performance OSCs and other optoelectronic devices.
[0197] It should be noted that, in this article, the terms "comprises", "includes" or any other variations are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements not explicitly listed. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the presence of other identical elements in the article or device including the elements. The orientation or positional relationship indicated by "upper", "lower", "left", "right", etc. is based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0198] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. An organic photovoltaic cell with a magnetic GO-doped hole transport layer, characterized in that: include: An ITO anode, a hole transport layer, an active layer, an electron transport layer and a metal cathode are arranged in sequence from bottom to top, wherein the material of the hole transport layer is magnetic GO-doped PEDOT:PSS.
2. The organic photovoltaic cell with a magnetic GO doped hole transport layer according to claim 1, characterized in that: The thickness of the hole transport layer is 20-30 nm.
3. The organic photovoltaic cell with a magnetic GO doped hole transport layer according to claim 1, characterized in that: The magnetic GO is a Fe3O4 / GO magnetic nanocomposite material.
4. The organic photovoltaic cell with a magnetic GO doped hole transport layer according to claim 1, characterized in that: The material of the active layer is PM6:L8-BO, and the thickness is 90-110nm.
5. The organic photovoltaic cell with a magnetic GO doped hole transport layer according to claim 1, characterized in that: The material of the electron transport layer is PNDIT-F3N, and the thickness is 5-10 nm.
6. A method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer, characterized in that: An organic photovoltaic cell applicable to the magnetic GO-doped hole transport layer according to any one of claims 1 to 5, wherein the preparation method comprises: Step 1: Surface pretreatment of ITO glass; Step 2: preparing a hole transport layer spin coating liquid, spin coating the hole transport layer spin coating liquid on the ITO glass after surface pretreatment by spin coating process, and then annealing to obtain a hole transport layer; wherein the material of the hole transport layer is magnetic GO-doped PEDOT:PSS; Step 3: preparing an active layer spin coating liquid, spin coating the active layer spin coating liquid on the hole transport layer by a spin coating process, and then performing annealing treatment to obtain an active layer; Step 4: preparing an electron transport layer spin coating liquid, and spin coating the electron transport layer spin coating liquid on the active layer by a spin coating process to obtain an electron transport layer; Step 5: Prepare a metal cathode on the electron transport layer by using an evaporation process.
7. The method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer according to claim 6, characterized in that: The step 1 comprises: Step 1.1: ultrasonically clean the ITO glass with deionized water, acetone, detergent, deionized water and isopropanol in sequence; Step 1.2: Drying the ITO glass after ultrasonic cleaning; Step 1.3: The dried ITO glass surface is treated with ozone plasma.
8. The method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer according to claim 6, characterized in that: The step 2 comprises: Step 2.1: Disperse the prepared Fe3O4 nanoparticles in an ethanol solution, add GO nanosheets to the mixed solution of Fe3O4 nanoparticles and ethanol, and load the Fe3O4 nanoparticles on the GO surface by stirring to form magnetic GO; Step 2.2: Dispersing magnetic GO in deionized water to obtain a magnetic GO aqueous solution with a concentration of 0.01-0.1 mg / ml; Step 2.3: Mixing the magnetic GO aqueous solution and PEDOT:PSS in a volume ratio of 1:1 to obtain the hole transport layer spin coating solution; Step 2.4: Spin coating the hole transport layer spin coating liquid onto the surface pretreated ITO glass using a spin coating process, and then perform annealing to obtain the hole transport layer, wherein the annealing temperature is 120-150° C. and the time is 10-20 min.
9. The method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer according to claim 6, characterized in that: The step 3 comprises: Step 3.1: PM6 and L8-BO in a mass ratio of 1:1.2 are dissolved in chloroform containing 0.3% DIO as an additive, and stirred at room temperature for 12 hours to obtain the active layer spin coating solution, wherein the total concentration of PM6 and L8-BO in the active layer spin coating solution is 13.2-16.5 mg / ml; Step 3.2: Spin-coat the active layer spin-coating liquid on the hole transport layer using a spin-coating process, and then perform annealing to obtain the active layer, wherein the annealing temperature is 90-120° C. and the time is 10-15 min.
10. The method for preparing an organic photovoltaic cell with a magnetic GO-doped hole transport layer according to claim 6, characterized in that: The step 4 comprises: Step 4.1: dissolving PNDIT-F3N in methanol containing 0.5% glacial acetic acid to obtain the electron transport layer spin coating solution, wherein the concentration of PNDIT-F3N in the electron transport layer spin coating solution is 0.5-1 mg / ml; Step 4.2: Spin-coating the electron transport layer spin-coating liquid on the active layer using a spin-coating process to obtain the electron transport layer.
Citation Information
Patent Citations
Preparation method of amino and carboxyl functionalized magnetic microsphere composite absorbent
CN109569544A
Non-fullerene acceptor material and preparation method and application thereof
CN116375732A
Organic solar cell and preparation method thereof
CN116801647A