Method for preparing flexible spin valve device
By preparing multilayer PI films on a PI carrier and utilizing laser-induced graphene technology, combined with antiferromagnetism and magnetic particles, the problem of unstable magnetic properties of flexible magnetic films under strain was solved, achieving efficient fabrication and improved stability of flexible spin valve devices.
Patent Information
- Application Number
- CN202410826451.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-25
AI Technical Summary
Flexible magnetic films exhibit unstable magnetic anisotropy when stretched or compressed, affecting device stability. Existing technologies struggle to maintain the stability of magnetic properties in flexible materials.
Using PI as a carrier and combining laser-induced graphene technology, multilayer PI films are prepared. Using antiferromagnetism and magnetic particles as dopants, flexible spin valve devices are fabricated, including a bottom electrode, an antiferromagnetic pinning layer, a fixed ferromagnetic electrode, a tunnel barrier layer, and a free ferromagnetic electrode. The electrode structure is formed by laser direct writing process.
This method improves the bending resistance of flexible spin valve devices, is simple to operate and has no mask contamination, and provides a new method for large-scale fabrication of flexible magnetic electronic devices.
Smart Images

Figure CN118900618A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetoelectronics, in particular to a method for preparing a flexible spin valve device. Background Art
[0002] With the development of the Internet of Things, wearable devices and bionic robotics, flexible electronic devices have begun to receive widespread attention. Among them, flexible magnetic electronic devices based on magnetic films can be integrated into smart wearable devices as sensors and memory units, and have important application prospects. There are two main methods for preparing flexible metal magnetic films: one is to obtain a self-supporting magnetic film through a sacrificial layer method and then transfer it to a flexible substrate; the other is to deposit a magnetic film directly on a flexible substrate. Common flexible substrates include: polyvinylidene fluoride (PVDF), polyimide (PI), polydimethylsiloxane (PDMS) and polyethylene terephthalate (PET), etc., among which a flat magnetic film can be directly grown on PET and PI. However, due to the influence of magnetoelastic anisotropy, the performance of flexible materials will be affected when stretched or compressed, which is not conducive to the stability of the device. Therefore, it is necessary to explore methods to enable flexible magnetic films to maintain magnetic anisotropy stability under strain.
[0003] Spin valves are one of the important devices in the field of spin electronics. They use electron spin rather than charge to manipulate current, thereby achieving more efficient magnetic storage and magnetic sensor devices. Flexible spin valves are spin electronic devices that can be bent and stretched. With the rise of flexible electronics around 2000, researchers began to explore the combination of flexible materials and spin, with a focus on the study of flexible magnetic materials. Preliminary experiments in 2006 showed the feasibility of depositing magnetic films on flexible substrates, laying the foundation for subsequent research on flexible spin valves. In 2010, flexible spin valves were successfully prepared. Spin valve structure films are usually deposited on flexible substrates of polyimide (PI) or polyparaxylene (Parylene). These flexible spin valves can maintain their giant magnetoresistance (GMR) or tunnel magnetoresistance (TMR) effects in a bent state. In 2025, researchers began to use two-dimensional materials and one-dimensional nanowires to manufacture flexible spin valves, significantly improving their performance. After that, research on flexible spin valves focused on their reliability or applications.
[0004] PI is a high-performance polymer material that has been widely used in many fields due to its excellent thermal stability, mechanical strength and chemical resistance. Laser-induced graphene (LIG) technology is an innovative method that directly converts certain carbon-containing materials into graphene through laser processing. This technology is fast, efficient, controllable and low-cost, and has shown broad application prospects in many fields. Materials that can respond to magnetic fields in some way are called magnetic materials. According to the strength of the material in the external magnetic field, it can be divided into diamagnetic, paramagnetic, ferromagnetic, antiferromagnetic and ferrimagnetic materials. For magnetic materials, magnetization curves and hysteresis loops are characteristic curves that reflect their basic magnetic properties. Ferromagnetic materials are generally Co, Fe, Ni elements and their alloys, rare earth elements and their alloys, and some Mn compounds. Magnetic materials are a typical class of functional materials. Their unique electromagnetic properties make them widely used in magnetic sensing, information processing and magnetic storage. Summary of the invention
[0005] The present invention proposes a method for preparing a flexible spin valve, using PI as a carrier, antiferromagnetic particles and magnetic particles as dopants to prepare a multilayer PI film, and combining the laser induced graphene (LIG) process to prepare a flexible spin valve device.
[0006] The technical solution provided by the present invention is as follows: A method for preparing a flexible spin valve device, comprising the steps of: 1) Preparation of bottom electrode: PI tape is pasted on the substrate, and a graphene bottom electrode is formed on the PI tape using a laser direct writing induced graphene process; 2) Preparation of the antiferromagnetic pinning layer, specifically including the following steps: 2-1) Mix the antiferromagnetic particles evenly into the PI liquid; 2-2) The above substrate is placed on a coating machine, and the PI liquid obtained in step 2-1) is dropped on the central area of the substrate, spin-coated, and cured to form a PI film on the graphene bottom electrode. 2-3) Performing laser direct writing operation to obtain a graphene layer containing antiferromagnetic particles as an antiferromagnetic pinning layer; since the graphene layer contains antiferromagnetic particles, the antiferromagnetic pinning layer can fix the magnetic moment direction of the fixed ferromagnetic electrode; 3) Preparation of fixed ferromagnetic electrodes, specifically including the following steps: 3-1) Evenly mix the ferromagnetic particles into the PI liquid; 3-2) placing the substrate on a coating machine, dropping the PI liquid obtained in step 3-1) on the central area of the substrate, performing spin coating, and curing treatment to form a PI film on the antiferromagnetic pinning layer, the thickness of which is less than the PI film prepared in step 2-2); 3-3) performing a laser direct writing operation to obtain a graphene layer containing ferromagnetic particles as a fixed ferromagnetic layer; 4) Preparation of tunnel barrier layer: Select pure PI liquid or dope PI liquid with non-magnetic insulating particles, then place the above substrate on a coating machine, drop pure PI liquid or PI liquid doped with non-magnetic insulating particles on the central area of the substrate, spin coat, and solidify to form a PI film on the fixed ferromagnetic layer, and use the PI film as the tunnel barrier layer; 5) Preparation of a free ferromagnetic electrode: using steps 3-1) to 3-3), a graphene layer containing ferromagnetic particles is obtained, and the graphene layer is used as a free ferromagnetic electrode layer; the thickness of the free ferromagnetic layer can be different from or the same as that of the fixed ferromagnetic layer, and the type of magnetic particles doped in the free ferromagnetic layer can be the same as or different from that in the fixed ferromagnetic layer; 6) Preparation of the top electrode: a layer of PI liquid is coated on the surface of the above substrate and cured to form a PI film on the free ferromagnetic layer. A laser direct writing process is used to obtain a graphene top electrode, thereby forming a device structure; 7) Packaging of spin valve devices: PI tape is used to stick flatly on the outer surface of the device structure. At the same time, the bottom layer of PI tape is separated from the rigid substrate. The bottom electrode and the top electrode are exposed using a laser direct writing process to obtain a flexible spin valve device.
[0007] Furthermore, in step 1), the substrate is glass, mica or silicon wafer.
[0008] Furthermore, the antiferromagnetic particles are CoFeB, CoO, MnAu, CrSb, Mn2As, NiMn, MnO, FeO, CoO, NiO, MnS, α-Fe2O3, FeS, FeCl2 or MnF2 particles.
[0009] Furthermore, the ferromagnetic particles are Fe, Co, Ni, FeCo, FeNi or CoFeB particles.
[0010] Furthermore, the non-magnetic insulating particles are MgO, Al2O3, AlN, TiO2 or ZnO particles.
[0011] Furthermore, in step 2-1), the ratio of antiferromagnetic particles to PI liquid is 0.1 g / mL to 0.3 g / m, and in step 3-1), the ratio of ferromagnetic particles to PI liquid is 0.1 g / mL to 0.3 g / m. The specific operation of uniformly mixing antiferromagnetic particles or ferromagnetic particles into PI liquid is as follows: first, an organic solvent is used as a dispersant, antiferromagnetic particles or magnetic particles are dissolved in the organic solvent, and then mixed with PI liquid, and ultrasonically placed in an ultrasonic container to obtain PI liquid uniformly doped with antiferromagnetic particles or magnetic particles, wherein the organic solvent is selected from one of dimethylformamide, dimethylacetamide or N-methylpyrrolidone.
[0012] Furthermore, the spin coating in step 2-2), step 3-2) or step 4) is specifically as follows: firstly, a low rotation speed is set to spread the PI liquid evenly, and then a high rotation speed is set to evenly distribute the PI liquid.
[0013] Furthermore, the curing in step 2-2), step 3-2) or step 4) is specifically divided into three stages, namely, the first stage: 60℃-100℃, keep for 20min-30min; the second stage: 150℃-200℃, keep for 40min-60min; the third stage: 260℃-300℃, keep for 30min-60min.
[0014] The beneficial effects of the present invention are as follows: The present invention prepares a flexible spin valve device. Since each layer of the film is a flexible material, its bending resistance is significantly improved. The present invention uses laser-induced graphene technology to directly write electrodes. The operation is simple and maskless, which effectively prevents the film from being contaminated. The spin valve preparation process of the present invention is simple and can be prepared on a large scale, providing a new idea for the preparation of magnetic electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The figure is a flow chart of the preparation of a spin valve according to a specific embodiment of the present invention.
[0016] Figure 2 These are characterization diagrams of graphene generated in a specific embodiment of the present invention, in which: (a) is an optical microscope image of graphene generated by laser direct writing of pure PI; and (b) is an optical microscope image of graphene generated by spin coating and solidification of PI liquid doped with ferromagnetic particles and then laser direct writing. DETAILED DESCRIPTION
[0017] The present invention is further described below by preparing a flexible CoFeB-MgO-CoFeB-IrMn spin valve. It should be noted that the purpose of publishing the embodiments is to help further understand the present invention, but those skilled in the art can understand that various substitutions and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the present invention should not be limited to the contents disclosed in the embodiments, and the scope of protection claimed by the present invention shall be subject to the scope defined in the claims.
[0018] like Figure 1 As shown, the method for preparing a flexible spin valve device of the present invention comprises the following specific steps: (1) Preparation of bottom electrode: Select a glass sheet of 5 cm × 5 cm in size, stick the PI tape flatly on the glass sheet, set the electrode shape to 50 um × 50 um, and directly pattern the PI tape to generate a graphene electrode, such as Figure 2 (a).
[0019] (2) Preparation of pinning layer: First, an organic solvent is used as a dispersant, such as dimethylformamide (DMF), dimethylacetamide (DMAC), and N-methylpyrrolidone (NMP). IrMn antiferromagnetic particles are dissolved in the organic solvent, and then mixed with PI. The mixture is placed in an ultrasonic container for 30 minutes to obtain a PI liquid uniformly doped with antiferromagnetic particles. The ratio of IrMn antiferromagnetic particles to PI is 0.6g / 4ml. The PI liquid is spin-coated on the center area of the glass sheet in two steps. First, a low speed is set to spread the PI liquid flat, and then a high speed is set to make the PI liquid evenly distributed. Then, vacuum heating is used for curing. The temperature is raised to 100°C and kept at a constant temperature for 30 minutes. Then, the temperature is raised to 150°C and kept at a constant temperature for 40 minutes. The temperature is further raised to 300°C and kept at a constant temperature for 30 minutes to 1 hour. The PI film is cured, and the cured PI film is subjected to laser direct writing to prepare graphene containing IrMn as an antiferromagnetic pinning layer.
[0020] (3) Preparation of a fixed ferromagnetic layer: Using the same method as step (2), the anti-ferromagnetic particles IrMn are replaced with magnetic particles CoFeB to obtain a PI liquid doped with magnetic particles CoFeB. Here, the thickness of the layer can be controlled to 1 / 4 of the thickness of the anti-ferromagnetic pinned layer by setting the speed of the coating machine. Then, a curing treatment is performed to prepare a PI film containing ferromagnetic particles. The PI film is subjected to a laser direct writing operation to obtain a graphene layer containing ferromagnetic particles as a fixed ferromagnetic layer, such as Figure 2 (b) shown.
[0021] (4) Preparation of tunnel barrier layer: Place a glass sheet on a coating machine and drop PI liquid doped with non-magnetic particles MgO on the center area of the glass sheet. The thickness of the layer can be controlled to be equivalent to the thickness of the fixed ferromagnetic layer by setting the rotation speed of the coating machine.
[0022] (5) Preparation of a free ferromagnetic layer: The PI liquid doped with magnetic particles CoFeB is obtained in the same manner as in step 3. The thickness of the layer can be controlled to be the same as the thickness of the fixed ferromagnetic layer by setting the rotation speed of the coating machine. Then, a laser direct writing operation is performed to obtain a graphene layer containing ferromagnetic particles. The graphene layer serves as a free ferromagnetic layer.
[0023] (6) Making a graphene top electrode: coating a layer of PI liquid on the upper surface of the free ferromagnetic layer and solidifying it, and then performing a laser direct writing operation to prepare a graphene top electrode. The two-terminal electrode structure provided in the present invention can increase the number of pad uses and the utilization rate of the device.
[0024] (7) Making the encapsulation layer: Finally, PI tape is used as the encapsulation layer. The PI tape is evenly pasted on the outer surface of the device structure, and the bottom layer of PI tape is separated from the rigid substrate. The PI tape is subjected to laser direct writing. The purpose of this laser direct writing process is only to expose the bottom electrode and the top electrode to the outside, and the other parts are protected by the PI film. After the preparation is completed, the electrode part and the PI layer with a width of 1um*1um are separated into many individual spin valve devices by laser cutting to realize mass production of the device. The flexible spin valve is obtained by the present invention. The structure can be used for magnetic storage and can also be used to measure magnetic variables.
[0025] The embodiments described above are not intended to limit the present invention. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention is defined by the scope of the claims.
Claims
1. A method for preparing a flexible spin valve device, comprising the steps of: 1) Preparation of bottom electrode: PI tape is pasted on the substrate, and a graphene bottom electrode is formed on the PI tape using a laser direct writing induced graphene process; 2) Preparation of the antiferromagnetic pinning layer, specifically including the following steps: 2-1) Mix the antiferromagnetic particles evenly into the PI liquid; 2-2) The above substrate is placed on a coating machine, and the PI liquid obtained in step 2-1) is dropped on the central area of the substrate, and spin-coated and cured to form a PI film on the graphene bottom electrode. 2-3) performing a laser direct writing operation to obtain a graphene layer containing antiferromagnetic particles as an antiferromagnetic pinning layer; 3) Preparation of fixed ferromagnetic electrodes, specifically including the following steps: 3-1) Evenly mix the ferromagnetic particles into the PI liquid; 3-2) placing the substrate on a coating machine, dropping the PI liquid obtained in step 3-1) on the central area of the substrate, performing spin coating, and curing treatment to form a PI film on the antiferromagnetic pinning layer, the thickness of which is less than the PI film prepared in step 2-2); 3-3) performing a laser direct writing operation to obtain a graphene layer containing ferromagnetic particles as a fixed ferromagnetic layer; 4) Preparation of tunnel barrier layer: Select pure PI liquid or dope PI liquid with non-magnetic insulating particles, then place the above substrate on a coating machine, drop pure PI liquid or PI liquid doped with non-magnetic insulating particles on the central area of the substrate, spin coat, and solidify to form a PI film on the fixed ferromagnetic layer, and use the PI film as the tunnel barrier layer; 5) Preparation of a free ferromagnetic layer: using steps 3-1) to 3-3), a graphene layer containing ferromagnetic particles is obtained, and the graphene layer serves as a free ferromagnetic layer; 6) Preparation of the top electrode: a layer of PI liquid is coated on the surface of the above substrate and cured to form a PI film on the free ferromagnetic layer. A laser direct writing process is used to obtain a graphene top electrode, thereby forming a device structure; 7) Packaging of spin valve devices: PI tape is used to stick flatly on the outer surface of the device structure. At the same time, the bottom layer of PI tape is separated from the rigid substrate. The bottom electrode and the top electrode are exposed using a laser direct writing process to obtain a flexible spin valve device.
2. The method according to claim 1, characterized in that The substrate in step 1) is glass, mica or silicon wafer.
3. The method according to claim 1, characterized in that The antiferromagnetic particles are CoFeB, CoO, MnAu, CrSb, Mn2As, NiMn, MnO, FeO, CoO, NiO, MnS, α-Fe2O3, FeS, FeCl2 or MnF2 particles.
4. The method according to claim 1, characterized in that The ferromagnetic particles are Fe, Co, Ni, FeCo, FeNi or CoFeB particles.
5. The method according to claim 1, characterized in that The non-magnetic insulating particles are MgO, Al2O3, AlN, TiO2 or ZnO particles.
6. The method according to claim 1, characterized in that In step 2-1), the ratio of antiferromagnetic particles to PI liquid is 0.1 g / mL~0.3 g / m, and in step 3-1), the ratio of ferromagnetic particles to PI liquid is 0.1 g / mL~0.3 g / m.
7. The method according to claim 1, characterized in that The specific operation of uniformly mixing antiferromagnetic particles or ferromagnetic particles into PI liquid is as follows: first, an organic solvent is used as a dispersant, the antiferromagnetic particles or magnetic particles are dissolved in the organic solvent, and then mixed with the PI liquid, and then placed in an ultrasonic container for ultrasonication to obtain a PI liquid uniformly doped with antiferromagnetic particles or ferromagnetic particles, wherein the organic solvent is selected from one of dimethylformamide, dimethylacetamide or N-methylpyrrolidone.
8. The method according to claim 1, characterized in that The spin coating in step 2-2), step 3-2) or step 4) is specifically as follows: firstly, a low rotation speed is set to spread the PI liquid evenly, and then a high rotation speed is set to evenly distribute the PI liquid.
9. The method according to claim 1, characterized in that The curing in step 2-2), step 3-2) or step 4) is specifically divided into three stages, namely, the first stage: 60°C-100°C, maintained for 20min-30min; the second stage: 150°C-200°C, maintained for 40min-60min; The third stage: 260℃-300℃, maintain for 30min-60min.
Citation Information
Patent Citations
Design method of ultra-thin spin valve device
CN110190182A
Spin valve film with synthetic anti-ferromagnetic structure
CN110416405A
Oxide giant magnet resistor spin valve, preparing process and its use
CN1512603A
Spin valve type thin-film magnetic element, thin-film magnetic head, floating magnetic head, and method for manufacturing the spin valve type thin-film magnetic element
JP2002140805A
Spin transfer magnetic elements with spin depolarization layers
US20050237787A1