Catalyst for producing carbon nanotubes and production method thereof
By supporting the catalyst composition on hydrotalcite, carbon nanotubes with large specific surface area and low powder resistance are prepared, which solves the problem of poor dispersion of carbon nanotubes and improves its performance and processability in electrode manufacturing.
Patent Information
- Application Number
- CN202380026571.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-28
- Filing Date
- 2023-10-26
- Publication Date
- 2024-11-05
AI Technical Summary
Carbon nanotubes are prone to aggregate in dispersions, resulting in poor dispersion and increased viscosity, affecting their processability and electrical conductivity in electrode manufacturing.
Using a catalyst composition supported on hydrotalcite, including a main catalyst component (such as Ni, Co, Fe) and a cocatalyst component (such as Mo, V), to prepare a large specific surface area and Low powder resistance carbon nanotubes.
The dispersion and processability of carbon nanotubes are improved, the viscosity is maintained, and it is suitable as a conductive material, which enhances its performance in electrode manufacturing.
Smart Images

Figure BDA0005035511110000081 
Figure BDA0005035511110000091
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Korean Patent Application No. 10-2022-0141852, filed on October 28, 2022, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] The present invention relates to a catalyst capable of synthesizing carbon nanotubes having a large specific surface area and low powder resistance and a preparation method thereof. Background Art
[0004] Carbon nanomaterials include fullerene, carbon nanotube (CNT), graphene and graphite nanosheet according to the shape of the material. Among them, carbon nanotube is a macromolecule in which a hexagonal honeycomb graphite surface (in which one carbon atom is bonded to three other carbon atoms) is rolled into a nanometer-sized diameter.
[0005] Carbon nanotubes are hollow and lightweight, and have electrical conductivity as good as copper, thermal conductivity as good as diamond, and tensile strength as good as steel. According to the winding form, they are also divided into single-walled carbon nanotubes (SWCNTs), multi-walled carbon nanotubes (MWCNTs), and rope-like carbon nanotubes.
[0006] Recently, the most active field of research on the use of carbon nanotubes is the field of lithium secondary batteries. The ultimate goal of lithium secondary batteries is to store more electrical energy in a smaller size. As one of the methods for manufacturing electrodes with higher energy density per unit volume by increasing the electrode density of lithium secondary batteries, a method of using carbon nanotubes as conductive materials is being studied. Generally, since high-density electrodes are formed by molding electrode active material particles with a size of several microns to tens of microns by a high-pressure press, the particles are easily deformed during the molding process, the space between the particles is reduced, and the electrolyte permeability is reduced. In order to solve this problem, materials with excellent conductivity and strength are used as conductive materials when manufacturing electrodes. Carbon nanotubes are also widely used as conductive materials because of their excellent strength and conductivity. When a conductive material is used in electrode manufacturing, the conductive material is dispersed between the compressed electrode active materials to maintain the micropores between the active material particles, thereby promoting the penetration of the electrolyte and reducing the resistance within the electrode due to excellent conductivity.
[0007] However, when using carbon nanotubes as a conductive material, the biggest problem is the low solubility and dispersibility of the carbon nanotubes themselves. The problem with carbon nanotubes is that they cannot achieve stable dispersion in an aqueous solution due to the strong van der Waals attraction between them, and aggregation occurs. If the carbon nanotubes aggregate in a dispersion, the workability of the dispersion deteriorates and the dispersion cannot be applied uniformly. Therefore, it is preferred to apply the dispersion in a state that minimizes the viscosity of the dispersion.
[0008] As a method for improving the poor dispersibility of carbon nanotube dispersion, various methods are known. For example, a method for dispersing carbon nanotubes in a dispersion medium by mechanical dispersion treatment such as ultrasonic treatment has been proposed. However, in the case of this method, the dispersibility when ultrasonic irradiation is excellent, but the carbon nanotubes begin to gather immediately after the ultrasonic irradiation is terminated, and even when the concentration of the carbon nanotubes is higher than a certain level, there is a problem of rapid aggregation of the carbon nanotubes. In addition, methods for dispersing and stabilizing carbon nanotubes using various dispersants have been proposed, but these methods also have the problem of being difficult to suppress the increase in viscosity that may occur when the carbon nanotubes are dispersed in a dispersion medium at a high concentration.
[0009] Therefore, there is a need to produce a new carbon nanotube in which the dispersibility can be further improved by improving the properties of the carbon nanotube itself rather than by a mechanical dispersion treatment such as ultrasonic treatment or an auxiliary means such as the use of a dispersant.
[0010] Prior art literature
[0011] (Patent Document 1) KR10-2017-0031061A (Publication Date: March 20, 2017) Summary of the invention
[0012] [Technical issues]
[0013] An object of the present invention is to provide a novel catalyst for producing carbon nanotubes and a method for producing the catalyst, wherein the catalyst is capable of producing carbon nanotubes which are particularly suitable for use as conductive materials due to their large specific surface area and low powder resistance, as well as their low viscosity when preparing dispersions and thus excellent processability.
[0014] [Technical solution]
[0015] In order to solve the above problems, the present invention provides a catalyst for producing carbon nanotubes and a preparation method thereof.
[0016] Specifically, (1) the present invention provides a catalyst for producing carbon nanotubes, which comprises a co-catalyst component and a main catalyst component supported on hydrotalcite, wherein the content of the main catalyst component is less than 10 weight % based on the total weight of the catalyst, and the molar ratio of the main catalyst component to the co-catalyst component is 1.0 to 10.
[0017] (2) The present invention provides the catalyst for producing carbon nanotubes according to (1) above, wherein the volume average particle size of the hydrotalcite is 10 μm to 200 μm.
[0018] (3) The present invention provides the catalyst for producing carbon nanotubes according to (1) or (2) above, wherein the main catalyst component is at least one selected from the group consisting of Ni, Co and Fe.
[0019] (4) The present invention provides the catalyst for producing carbon nanotubes according to any one of (1) to (3) above, wherein the co-catalyst component is at least one selected from the group consisting of Mo and V.
[0020] (5) The present invention provides the catalyst for producing carbon nanotubes according to any one of (1) to (4) above, wherein the content of the main catalyst component is 5.0 wt% to 6.5 wt%.
[0021] (6) The present invention provides the catalyst for producing carbon nanotubes according to any one of (1) to (5) above, wherein the molar ratio of the main catalyst component to the co-catalyst component is 2.5 to 5.0.
[0022] (7) The present invention provides a method for preparing a catalyst for producing carbon nanotubes, the method comprising the following steps: preparing a catalyst composition (S1) by adding a co-catalyst precursor, a main catalyst precursor and an organic acid to a solvent; adding hydrotalcite to the catalyst composition, and drying and calcining it to obtain a catalyst (S2), wherein the molar ratio of the main catalyst precursor to the co-catalyst precursor added in step (S1) is 1.0 to 10, and the calcination is carried out at 150°C to 450°C.
[0023] (8) The present invention provides a method for preparing a catalyst for producing carbon nanotubes according to (7) above, wherein the molar ratio of the organic acid added in step (S1) to the co-catalyst precursor is 0.30 to 0.50.
[0024] (9) The present invention provides a method for preparing a catalyst for producing carbon nanotubes according to (7) or (8) above, wherein the molar ratio of the main catalyst precursor to the organic acid added in step (S1) is 7.0 to 12.0.
[0025] (10) The present invention provides a method for preparing a catalyst for producing carbon nanotubes according to any one of (7) to (9) above, wherein the calcination is performed at 150°C to 300°C.
[0026] [Beneficial Effects]
[0027] The carbon nanotubes synthesized using the catalyst of the present invention have a large specific surface area and low powder resistance, so when used as a dispersion, the viscosity of the dispersion itself can be kept low while the content of the carbon nanotubes is kept above a certain level. Therefore, the carbon nanotubes are particularly suitable for use as a conductive material. DETAILED DESCRIPTION
[0028] Hereinafter, the present invention will be described in more detail.
[0029] The terms or words used in the specification and claims of the present application should not be construed as limited to their general meanings or dictionary meanings, but should be construed as meanings and concepts consistent with the technical spirit of the present invention based on the principle that the inventor can fully define the concepts of the terms to best describe his invention.
[0030] The term "carbon nanotube" used in the present invention is a secondary structure formed by forming a bundle of carbon nanotube units in whole or in part, wherein the carbon nanotube unit has a graphite sheet in the shape of a cylinder with a nanometer-sized diameter and has an sp2 bond structure. In this case, the characteristics of a conductor or a semiconductor can be manifested according to the angle and structure of the winding of the graphite surface. According to the number of bonds forming the wall, the carbon nanotube unit can be divided into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT) and multi-walled carbon nanotubes (MWCNT), wherein the thinner the wall thickness, the lower the resistance.
[0031] The carbon nanotubes of the present invention may include one or more of single-walled, double-walled and multi-walled carbon nanotube units.
[0032] Catalysts for the production of carbon nanotubes
[0033] The present invention relates to a catalyst capable of synthesizing carbon nanotubes having a wide specific surface area and low powder resistance by using hydrotalcite having a hydroxyl group on the surface as a carrier and optimizing the molar ratio between the supported co-catalyst component and the main catalyst component and the content of the main catalyst component based on the total weight of the catalyst. More specifically, the present invention provides a catalyst for preparing carbon nanotubes, the catalyst comprising a co-catalyst component and a main catalyst component supported on hydrotalcite, wherein the content of the main catalyst component based on the total weight of the catalyst is 10% by weight or less, and the molar ratio of the main catalyst component to the co-catalyst component is 1.0 to 10.
[0034] Hereinafter, each component of the catalyst for producing carbon nanotubes according to the present invention will be described separately.
[0035] Hydrotalcite
[0036] Hydrotalcite is used as a carrier of the catalyst for producing carbon nanotubes of the present invention, and is characterized by having a structure containing magnesium and aluminum and having hydroxyl groups on the surface. Hydrotalcite has the following technical advantages, when it is applied to a supported catalyst, it is easy to impregnate a metal precursor due to the hydroxyl groups on the surface, and also has excellent durability.
[0037] Meanwhile, the volume average particle size of the hydrotalcite may be 10 μm to 200 μm, preferably 20 μm to 100 μm. In addition, the BET specific surface area of the hydrotalcite may be 1 m 2 / g to 100m 2 / g, 5m 2 / g to 50m 2 / g, preferably 12m 2 / g to 40m 2 / g.
[0038] When the volume average particle diameter and the specific surface area of the hydrotalcite are within the above ranges, the co-catalyst and the main catalyst components described below can be effectively supported, and the carbon nanotubes produced using the catalyst can have a large specific surface area.
[0039] The shape of the hydrotalcite is not particularly limited, but may be spherical or potato-shaped. In addition, the hydrotalcite may have a porous structure, a molecular sieve structure, a honeycomb structure, etc., to have a relatively high surface area per unit mass or unit volume.
[0040] Main catalyst component
[0041] In the catalyst for producing carbon nanotubes of the present invention, the main catalyst component can be one or more selected from Ni, Co and Fe, preferably Co. The main catalyst component is used to promote the carbon nanotube synthesis reaction by directly reducing the activation energy of the reaction of synthesizing carbon nanotubes from carbon source gas. When using the above main catalyst component, it is desirable that the manufactured catalyst can have high activity and durability can also be ensured above a certain level.
[0042] In the catalyst for producing carbon nanotubes of the present invention, the content of the main catalyst component can be 10 weight % or less, preferably 5.0 weight % to 6.5 weight %. Even if the content of the main catalyst component is higher than the above range, the improvement of the catalytic activity is not significant, and if the content of the main catalyst component is too low, the activity of the catalyst itself may be greatly reduced. In particular, in the case of the prior art, it is disclosed that the catalytic activity is maximized by increasing the content of the main catalyst component to exceed the above range. However, as will be described below, when the main catalyst content is 10 weight % or less and the molar ratio of the main catalyst component to the co-catalyst component is 1.0 to 10, sufficient catalytic activity can be exhibited, and the specific surface area of the produced carbon nanotubes can be increased.
[0043] Co-catalyst component
[0044] In the catalyst for producing carbon nanotubes of the present invention, the co-catalyst component may be one or more selected from Mo and V, preferably V. The co-catalyst component plays a role in further improving the catalytic activity of the main catalyst component. When the above-mentioned co-catalyst component is used, the synergistic effect with the main catalyst component may be excellent, and aggregation between the main catalyst components during the manufacturing process may be prevented.
[0045] In the catalyst for producing carbon nanotubes of the present invention, the molar ratio of the main catalyst component to the co-catalyst component can be 1.0 to 10, preferably 2.5 to 5.0. By setting the ratio between the main catalyst component and the co-catalyst component within the above range, sufficient catalytic activity can be achieved through the synergistic effect between the main catalyst component and the co-catalyst component without unnecessarily increasing the main catalyst content.
[0046] Method for producing a catalyst for producing carbon nanotubes
[0047] The present invention provides a method for producing the above-mentioned catalyst for producing carbon nanotubes. Specifically, the present invention provides a method for preparing a catalyst for producing carbon nanotubes, the method comprising the following steps: preparing a catalyst composition (S1) by adding a co-catalyst precursor, a main catalyst precursor and an organic acid to a solvent; adding hydrotalcite to the catalyst composition, and drying and calcining it to obtain a catalyst (S2), wherein the molar ratio of the main catalyst precursor to the co-catalyst precursor added in step (S1) is 1.0 to 10, and the calcination is carried out at 150°C to 450°C.
[0048] Hereinafter, each step of the above-mentioned manufacturing method will be described separately.
[0049] Step of preparing a catalyst composition (S1)
[0050] The main catalyst precursor used in this step is a component for introducing the main catalyst component into the above-mentioned catalyst, and can be a compound containing the main catalyst component. More specifically, the main catalyst precursor can be a salt or oxide of Fe, Ni and Co, or a compound containing the metal component, and particularly preferably can be a precursor based on Fe, Ni or Co, for example, Fe(NO3)2·6H2O, Fe(NO3)2·9H2O, Fe(NO3)3, Fe(OAc)2, Ni(NO3)2·6H2O, Co(NO3)2·6H2O, Co2(CO)8, [Co2(CO)6(t-BuC=CH)], Co(OAc)2.
[0051] The promoter precursor used in this step is a component for introducing the promoter component into the above-mentioned catalyst, and may be a compound containing the promoter component. The promoter precursor may also be a salt or oxide of V and Mo, or a compound containing the metal component, and particularly preferably, may be such as NH4VO3, (NH4)6Mo7O 24 · Materials of 4H2O, Mo(CO)6 or (NH4)MoS4. When the above-exemplified materials are used as precursors, there is an advantage in that the main catalyst component and the co-catalyst component are smoothly supported.
[0052] Meanwhile, like the molar ratio of the main catalyst component to the co-catalyst component in the catalyst, the molar ratio of the main catalyst precursor to the co-catalyst precursor in the catalyst composition may also be 1.0 to 10, preferably 2.5 to 5.0.
[0053] The organic acid can be, for example, a polycarboxylic acid, which is a compound containing two or more carboxyl groups, and has high solubility as a complexing agent, inhibits precipitation, promotes the synthesis of the catalyst, and acts as an activator to increase the synthesis of carbon nanotubes. The polycarboxylic acid can be one or more selected from dicarboxylic acids, tricarboxylic acids, and tetracarboxylic acids. For example, carboxylic acid compounds such as citric acid, oxalic acid, malonic acid, succinic acid, or tartaric acid, or anhydrides thereof can be used.
[0054] Depending on the amount of the organic acid added, the characteristics of the catalyst finally produced can vary. In the present invention, the amount of organic acid added is determined so that the molar ratio of the organic acid added in step (S1) to the co-catalyst precursor is 0.30 to 0.50, and the molar ratio of the main catalyst precursor added in step (S1) to the organic acid is 7.0 to 12.0. Within the input amount range of the organic acid as described above, the metal components of the main catalyst and the co-catalyst do not precipitate in the catalyst composition, and the occurrence of cracks can also be suppressed in the subsequent calcination process.
[0055] The solvent of the catalyst composition is not particularly limited as long as it can dissolve the above-mentioned main catalyst precursor and co-catalyst precursor, and for example, water is preferably used.
[0056] In the method for producing a catalyst for producing carbon nanotubes according to the present invention, it may further include a step of mixing the catalyst composition and aging it for a certain time before adding the hydrotalcite to the prepared catalyst composition. Specifically, the mixing may be performed by rotating or stirring at a temperature of 45° C. to 80° C. The aging may be performed for 3 to 60 minutes.
[0057] Drying and calcining step (S2)
[0058] The hydrotalcite as a carrier can be added to the catalyst composition prepared by the previous step so that the main catalyst and the co-catalyst component are supported in the carrier. Then, the main catalyst precursor and the co-catalyst precursor can be converted into the main catalyst component and the co-catalyst component by drying and calcining processes.
[0059] The drying in this step may be performed at 60° C. to 200° C. for 4 to 16 hours, and the drying method may be a conventional drying method used in the art, such as oven drying, reduced pressure drying, and freeze drying.
[0060] The calcination in this step can be carried out at a temperature of 150° C. to 450° C., preferably 150-300° C. In the conventional method for preparing a supported catalyst, the calcination is carried out at a temperature range much higher than the calcination temperature range of the present invention, but in the present invention, the calcination is carried out at the low temperature range. When the calcination is carried out in this temperature range, most of the main catalyst precursor and the co-catalyst precursor can be converted into the main catalyst component and the co-catalyst component, while minimizing the structural collapse of the hydrotalcite as a carrier.
[0061] Hereinafter, the present invention will be described in more detail by examples and experimental examples to specifically illustrate the present invention, but the present invention is not limited to these examples and experimental examples. However, embodiments according to the present invention may be modified in various forms, and the scope of the present invention should not be construed as being limited to the embodiments described in detail below. Embodiments of the present invention are provided in order to more completely explain the present invention to those skilled in the art.
[0062] Examples and Comparative Examples
[0063] Co(NO3)2·6H2O is used as a cobalt precursor, and NH4VO3 is used as a vanadium precursor. The catalyst composition is prepared by dissolving the cobalt precursor and the vanadium precursor in water and dissolving citric anhydride (CA) with an organic acid. The catalyst composition is fully stirred and then added to the hydrotalcite as a carrier. Then, it is dried at 190°C for 5 hours using an oven, and then calcined at a specific calcination temperature and in the atmosphere for 4 hours to complete the catalyst. In the above method, the amount of vanadium added is 0.3 molar ratio relative to 1 mole of cobalt, and the amount of citric anhydride is 0.13 molar ratio relative to 1 mole of cobalt. In the above method, various catalysts are prepared by changing the type of carrier, the cobalt content in the catalyst precursor composition, the ratio of cobalt to vanadium, the ratio of citric anhydride to vanadium, the calcination temperature, etc., and the catalyst preparation conditions in each embodiment and comparative example are summarized in Table 1 below.
[0064] [Table 1]
[0065]
[0066] Experimental Example 1. Confirmation of the properties of carbon nanotubes produced using the catalysts of Examples / Comparative Examples
[0067] The carbon nanotubes were synthesized using the catalyst prepared in the above embodiment. Specifically, after 0.3 g of the prepared catalyst was filled in a fixed bed reactor, nitrogen was injected into the fixed bed reactor at 1600 sccm, and the temperature in the reactor was heated to 670°C. Then, ethylene gas as a carbon source gas was injected at 400 sccm, and the reaction was continued for 90 minutes to synthesize carbon nanotubes. The yield, purity, specific surface area, bulk density and powder resistance of the synthesized carbon nanotubes were measured, and each property was measured using the following method.
[0068] 1) The yield was calculated by measuring the weight of the carbon nanotubes obtained by the reaction and using the following formula.
[0069] Yield = {(mass of recovered carbon nanotubes - mass of added catalyst) / (mass of added catalyst)}
[0070] 2) Purity: (amount of carbon nanotubes obtained - amount of catalyst added) / amount of carbon nanotubes obtained * 100%
[0071] 3) The specific surface area was calculated by measuring the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77 K) using BELSORP-mini II from BEL Japan.
[0072] 4) The bulk density was calculated by measuring the weight of the carbon nanotubes contained in the container freely falling using a 25 ml SUS measuring cup and dividing the measured weight by the volume of the container.
[0073] 5) When the compression density was 1 g / cc, the powder resistance was measured by measuring the resistance according to pressure using MCP-PD51 equipment from Nittoseiko Analytech.
[0074] The measurement results are summarized in Table 2 below.
[0075] [Table 2]
[0076]
[0077] As can be seen from Table 2 above, it can be confirmed that when the catalyst of the present invention is used, carbon nanotubes having a large specific surface area and a low powder resistance are synthesized.
[0078] More specifically, compared with the embodiment of the present invention, Comparative Examples 1-1 and 1-2 use a catalyst with a larger content of the main catalyst component. However, when a larger amount of the main catalyst component is loaded, the yield increases, which is substantially similar to the yields of each of the embodiments 1-7 using 8.5% by weight of the main catalyst component content or the embodiments 1-8 using 10% by weight of the main catalyst component content, but the specific surface area and the powder resistance are lower than the specific surface area and the powder resistance of the embodiment. It can be confirmed that even within the range of less than 10% by weight of the main catalyst component content, carbon nanotubes with a wider specific surface area and excellent electrical properties can be manufactured, and with respect to the performance of the carbon nanotubes, it is not ideal to increase the main catalyst component content to exceed this range.
[0079] In addition, in the case of Examples 2-1 to 2-2 in which the temperature in the calcination step is changed, although calcination is carried out at a temperature range significantly lower than the existing calcination temperature, the produced carbon nanotubes have a large specific surface area, low powder resistance, and satisfactory results in terms of yield and purity.
[0080] In the case of Comparative Examples 4-1 and 4-2 using alumina or magnesia instead of the hydrotalcite of the present invention as a carrier, the produced carbon nanotubes showed lower specific surface area, significantly high powder resistance, and significantly worse results in yield and purity compared with the Examples.
[0081] Furthermore, even in the case of Comparative Examples 4-3 and 4-4 in which hydrotalcite was used as a carrier but the molar ratio between Co (main catalyst component) and V (co-catalyst component) was too low or too high, carbon nanotubes having a lower specific surface area were produced compared to the case of using the catalysts of Examples 4-1 to 4-5 in which the same Co content was used but the molar ratio between Co and V was appropriate.
[0082] From the above results, it was confirmed that when the catalyst prepared by the catalyst preparation method of the present invention was used, carbon nanotubes having a large specific surface area and a low powder resistance could be synthesized.
Claims
1. A catalyst for producing carbon nanotubes, the catalyst comprising a co-catalyst component and a main catalyst component supported on hydrotalcite, in, The content of the main catalyst component is 10 wt% or less based on the total weight of the catalyst, and The molar ratio of the main catalyst component to the co-catalyst component is 1.0 to 10.
2. The catalyst for producing carbon nanotubes according to claim 1, wherein The volume average particle size of the hydrotalcite is 10 μm to 200 μm.
3. The catalyst for producing carbon nanotubes according to claim 1, wherein The main catalyst component is at least one selected from the group consisting of Ni, Co and Fe.
4. The catalyst for producing carbon nanotubes according to claim 1, wherein The co-catalyst component is at least one selected from the group consisting of Mo and V.
5. The catalyst for producing carbon nanotubes according to claim 1, wherein The content of the main catalyst component is 5.0 wt% to 6.5 wt%.
6. The catalyst for producing carbon nanotubes according to claim 1, wherein The molar ratio of the main catalyst component to the co-catalyst component is 2.5 to 5.
0.
7. A method for preparing a catalyst for producing carbon nanotubes, the method comprising the following steps: preparing a catalyst composition (S1) by adding a co-catalyst precursor, a main catalyst precursor and an organic acid to a solvent; as well as adding hydrotalcite to the catalyst composition, and drying and calcining it to obtain a catalyst (S2), Wherein, the molar ratio of the main catalyst precursor to the co-catalyst precursor added in step S1 is 1.0 to 10, and The calcination is performed at 150°C to 450°C.
8. The method for preparing a catalyst for producing carbon nanotubes according to claim 7, wherein: The molar ratio of the organic acid added in step S1 to the co-catalyst precursor is 0.30 to 0.
50.
9. The method for preparing a catalyst for producing carbon nanotubes according to claim 7, wherein: The molar ratio of the main catalyst precursor to the organic acid added in step S1 is 7.0 to 12.
0.
10. The method for preparing a catalyst for producing carbon nanotubes according to claim 7, wherein: The calcination is performed at 150°C to 300°C.
Citation Information
Patent Citations
Preparation method of array carbon nanotube supported catalyst
CN114029047A
BI-LAYER CATALYST, ITS PREPARATION PROCESS AND ITS USE IN THE MANUFACTURE OF NANOTUBS
FR2949074A1
CNT and method for manufacturing thereof
KR1020130082460A
Process for preparing aggregates of carbon nanotubes
KR1020160036910A
Method for preparing single walled carbon nanotubes
US20060239893A1