Coated tool and cutting tool

By using cubic crystal coating and multi-layer structure in coated tools, the problem of abnormal wear of existing tools in cutting processing is solved, and higher wear resistance and collapse resistance are achieved, which extends the tool life and Reduces wear.

CN118900738APending Publication Date: 2024-11-05KYOCERA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023712.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-07
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing coated tools have abnormal wear problems in cutting processing, which is difficult to effectively suppress primary boundary wear, secondary boundary wear and crescent wear, affecting tool life and processing accuracy.

Method used

A cubic crystal coating layer composed of selected elements in periodic laws 4a, 5a, 6a elements, Al, Si, B, Y, C, N, and a multi-layer structure combining layer, intermediate layer and wear-resistant layer , the coating layer is formed by physical evaporation method to ensure the consistent crystal orientation and the film thickness are between 2.5 μm and 10 μm, and the wear resistance and collapse resistance of the tool are improved.

Benefits of technology

It effectively suppresses abnormal wear, improves the wear and collapse resistance of the tool, extends the tool life, and reduces abrasive wear and boundary damage during cutting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900738A_ABST
    Figure CN118900738A_ABST
Patent Text Reader

Abstract

The coated cutting tool according to the present invention is provided with a base body and a coating layer on the surface of the base body. The coating layer contains cubic crystals comprising at least one element selected from among elements of groups 4a, 5a, 6a of the periodic law, Al, Si, B, Y, and Mn, and at least one element selected from among C and N. The difference between the maximum value and the minimum value of the X-ray intensity in the range where the angle of the alpha-axis is 30-90 degrees is 10% or less of the maximum value in the measurement range of 0-90 degrees inclusive in the Z-ray intensity distribution of the alpha-axis in the positive electrode diagram of the (111) plane of the coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a coated tool and a cutting tool. Background Art

[0002] As a tool used for cutting such as turning and milling, there is known a coated tool in which the surface of a base body such as cemented carbide, cermet, ceramic, etc. is coated with a coating layer to improve wear resistance and the like.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2019 / 146710

[0006] Patent Document 2: International Publication No. 2011 / 016488

[0007] Patent Document 3: International Publication No. 2010 / 007958 Summary of the invention

[0008] A coated tool according to one embodiment of the present invention comprises a substrate and a coating layer located on the surface of the substrate. The coating layer contains cubic crystals composed of at least one element selected from the periodic table 4a, 5a, 6a group elements, Al, Si, B, Y and Mn, and at least one element selected from C and N. In the measurement range of 0° to 90° of the X-ray intensity distribution of the α-axis of the positive pole diagram of the coating layer with respect to the (iii) surface, the difference between the maximum value and the minimum value of the X-ray intensity in the range of 30′ to 90′ is less than 10% of the maximum value. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 This is a perspective view showing an example of a coated tool according to the embodiment.

[0010] Figure 2 This is a side sectional view showing an example of a coated tool according to the embodiment.

[0011] Figure 3 It is a schematic enlarged view of a corner portion in the insert body of the reference example.

[0012] Figure 4 This is a cross-sectional view showing an example of a coating layer according to an embodiment.

[0013] Figure 5 This is a front view showing an example of a cutting tool according to an embodiment.

[0014] Figure 6This is a graph showing the X-ray intensity distribution of the positive pole figure of the cubic crystal contained in the coating layer with respect to the (111) plane.

[0015] Figure 7 This is a graph showing the X-ray intensity distribution of the positive pole figure of the cubic crystal contained in the coating layer with respect to the (200) plane.

[0016] Figure 8 This is a graph showing the correlation between the crystallite diameter in the (200) plane of the wear-resistant layer and the primary boundary wear amount.

[0017] Fig. 9 This is a graph showing the correlation between the Vickers hardness of the wear-resistant layer and the secondary boundary wear amount.

[0018] Fig.10 This is a graph showing the correlation between the Ti ratio (a) of the wear resistant layer and the primary boundary wear amount.

[0019] Fig.11 This is a graph showing the correlation between the Al ratio (b) of the wear-resistant layer and the primary boundary wear amount.

[0020] Fig.12 This is a graph showing the correlation between the Cr ratio (c) of the wear-resistant layer and the primary boundary wear amount.

[0021] Fig.13 This is a graph showing the correlation between the peeling load and the secondary boundary wear amount.

[0022] Fig.14 : is a graph showing the correlation between the Ti ratio (x) of the bonding layer and the peeling load.

[0023] Fig.15 : is a graph showing the correlation between the Al ratio (y) of the tie layer and the peeling load.

[0024] Fig.16 Graph showing the correlation between the Ti ratio (x) of the bonding layer and the secondary boundary wear amount.

[0025] Fig.17 Graph showing the correlation between the Al ratio (y) of the bonding layer and the secondary boundary wear amount.

[0026] Fig.18 This is a graph showing the correlation between the Ti ratio (e) of the intermediate layer and the crater wear depth.

[0027] Fig.19 This is a graph showing the correlation between the Al ratio (f) of the intermediate layer and the crater wear depth.

[0028] Fig. 20The images show the state of the cutting edge of three coated cutting tools having different film structures after the cutting test.

[0029] Fig.21 The images show the state of the cutting edge of eight coated cutting tools having different bonding layer compositions after the cutting test.

[0030] Fig. 22 The images show the state of the cutting edge of seven coated cutting tools having different compositions of the wear-resistant layer after the cutting test.

[0031] Fig.23 This is a graph showing the relationship between the film thickness of the wear-resistant layer and the amount of abrasive wear.

[0032] Fig.24 This is a graph showing the relationship between the film formation time of the tie layer and various wear amounts.

[0033] Fig.25 This is a graph showing the relationship between the film formation time of the tie layer and the number of impacts until the layer is broken.

[0034] Fig.26 This is an image obtained by photographing the state of the cutting edge of a sample having an intermediate layer after a cutting test from a direction perpendicular to the rake face.

[0035] Fig. 27 This is an image obtained by photographing the state of the cutting edge of a sample having no intermediate layer after a cutting test from a direction perpendicular to the rake face.

[0036] Fig.28 This is a table that summarizes the film thicknesses of the intermediate layer and the wear-resistant layer of five samples having different film thickness ratios of the intermediate layer and the wear-resistant layer, and images showing the state of the cutting edge after the cutting test. DETAILED DESCRIPTION

[0037] The following is a detailed description of the method for implementing the coated tool and cutting tool based on the present invention (hereinafter, recorded as "implementation method") with reference to the accompanying drawings. It should be noted that the coated tool and cutting tool based on the present invention are not limited by this embodiment. In addition, each embodiment can be appropriately combined within the scope of not making the processing content contradictory. In addition, the same reference numerals are marked on the same parts in the following embodiments, and repeated descriptions are omitted.

[0038] In the above-mentioned conventional technology, there is room for further improvement in terms of suppressing abnormal wear. Therefore, it is desired to provide a coated tool and a cutting tool that can suppress abnormal wear.

[0039] Figure 1 : is a perspective view showing an example of a coated tool according to an embodiment. Figure 21 is a side sectional view showing an example of a coated tool according to an embodiment. Figure 1 As shown, a coated tool 1 according to the embodiment includes an insert body 2 .

[0040] (Blade body 2)

[0041] The blade body 2 has, for example, an upper surface and a lower surface ( Figure 1 The shape of the surface (the surface intersecting the Z axis shown) is a parallelogram hexahedron.

[0042] A corner portion 201 of the blade body 2 functions as a cutting edge portion. The cutting edge portion has a first surface (e.g., an upper surface) and a second surface (e.g., a side surface) connected to the first surface. In an embodiment, the first surface functions as a "front face" for scraping off chips generated by cutting, and the second surface functions as a "flank face". A cutting edge is disposed on at least a portion of the ridgeline where the first surface and the second surface intersect, and the coated tool 1 cuts the cut material by pressing the cutting edge against the cut material.

[0043] A through hole 5 is disposed in the center of the blade body 2, penetrating the blade body 2 in the vertical direction. A screw 75 (see FIG. 1 ) for attaching the coated tool 1 to a tool holder 70 described later is inserted into the through hole 5. Figure 5 ).

[0044] like Figure 2 As shown, the insert body 2 has a base body 10 and a coating layer 20 .

[0045] (Substrate 10)

[0046] The substrate 10 is made of cemented carbide. Specifically, the substrate 10 includes a hard phase containing at least WC (tungsten carbide) and a metal binder phase containing an iron group element such as Ni (nickel) or Co (cobalt). As an example, the substrate 10 is composed of a WC-based cemented carbide, which uses hard particles composed of WC as a hard phase component and Co as a main component of the binder phase.

[0047] (Coating layer 20)

[0048] The coating layer 20 is applied to the substrate 10 for the purpose of improving the wear resistance, heat resistance, etc. of the substrate 10. Figure 2 In the example of , the coating layer 20 coats the substrate 10 as a whole. This example is not limited to the present example, and the coating layer 20 may be at least located on the substrate 10. When the coating layer 20 is located on the first surface (here, the upper surface) of the substrate 10, the wear resistance and heat resistance of the first surface are high. When the coating layer 20 is located on the second surface (here, the side surface) of the substrate 10, the wear resistance and heat resistance of the second surface are high.

[0049] (About the Pole Diagram)

[0050] The coating layer 20 of the embodiment may also contain cubic crystals composed of at least one element selected from the periodic table group 4a, 5a, 6a elements, Al, Si, B, Y and Mn, and at least one element selected from C, N and O. For example, the coating layer 20 may also contain cubic crystals composed of TiAlN. In this case, the coating layer 20 of the embodiment has a measurement range of more than 0° and less than 90° in the X-ray intensity distribution of the α-axis of the positive pole diagram of the cubic crystal with respect to the (111) plane, and the difference between the maximum value (Imax) and the minimum value (Imin) of the X-ray intensity in the range of more than 30° and less than 90° of the α-axis may also be less than 10% of the maximum value (Imax). The coating layer 20 having this structure has a homogeneous structure with a consistent crystal orientation, so that, for example, abnormal wear such as collapse can be suppressed.

[0051] In addition, the coating layer 20 of the embodiment may have a maximum value (Ilmax) and a minimum value (Ilmin) of X-ray intensity within a measurement range of 0° to 90° in the X-ray intensity distribution of the α-axis of the positive pole diagram of the (200) plane of the cubic crystal, and may also have a maximum value (Ilmax) and a minimum value (Ilmin) of X-ray intensity within a range of 0° to 50° in the α-axis angle. In this case, the difference between the maximum value (Ilmax) and the minimum value (Ilmin) may also be less than 10% relative to the maximum value (Ilmax). The coating layer 20 having this structure has a homogeneous structure with a consistent crystal orientation, so that, for example, abnormal wear such as collapse can be suppressed.

[0052] (About the damage mode of the blade body)

[0053] Here, refer to Figure 3 The manner in which damage occurs to the blade body will be described. Figure 3 It is a schematic enlarged view of a corner portion 201X in a blade body 2X of a reference example.

[0054] like Figure 3 As shown, the insert body 2X may generate primary boundary wear D1, secondary boundary wear D2, abrasive wear D3, and crater wear D4, for example. The primary boundary wear D1, secondary boundary wear D2, and abrasive wear D3 are wear generated on the back face. The crater wear D4 is wear generated on the front face.

[0055] The abrasive wear D3 is wear caused by scraping off the surface of the insert body 2X due to foreign matter interposed between the insert body 2X and the workpiece. The abrasive wear D3 may cause an increase in cutting resistance and cutting heat.

[0056] The primary boundary wear D1 and the secondary boundary wear D2 are wear produced at both ends of the abrasive wear D3, i.e., at the cut-in boundary. The primary boundary is the boundary that contacts the cut surface of the cut material. The secondary boundary is the boundary that contacts the finished surface of the cut material. The primary boundary wear D1 may cause burrs to the cut material. The secondary boundary wear D2 may deteriorate the finished surface of the cut material or change the size of the cut material.

[0057] The crater wear D4 is caused by the surface oxidation of the insert body 2X at a high temperature, thereby generating relatively soft oxides. The crater wear D4 may deteriorate chip handling performance.

[0058] The coated cutting tool 1 of the embodiment can appropriately suppress these damage modes by devising a structure of the coating layer 20 that coats the insert body 2 .

[0059] Here, refer to Figure 4 An example of the structure of the coating layer 20 according to the embodiment will be described. Figure 4 It is a cross-sectional view showing an example of the coating layer 20 according to the embodiment.

[0060] like Figure 4 As shown, the coating layer 20 has a bonding layer 21, an intermediate layer 22, and a wear-resistant layer 23. The bonding layer 21 is a layer in contact with the substrate 10. The intermediate layer 22 is located on the surface of the bonding layer 21. The wear-resistant layer 23 is located on the surface of the intermediate layer 22. That is, the bonding layer 21, the intermediate layer 22, and the wear-resistant layer 23 are stacked in the order of the bonding layer 21, the intermediate layer 22, and the wear-resistant layer 23 from the layer close to the surface of the substrate 10.

[0061] The bonding layer 21 is composed of Ti x Al y M z alloy layer. It should be noted that M is at least one metal selected from the 4a, 5a, 6a groups of the periodic table and Si. x and y are both 40≤x≤80, 0≤y≤55 in atomic ratio, and x+y+z=100. As an example, the bonding layer 21 may also be TiAlWNbSi. In addition, z may also be 0. That is, the bonding layer 21 does not necessarily need to contain M. In this case, the bonding layer 21 may also be TiAl, for example.

[0062] The wear-resistant layer 23 includes Ti a Al b Cr c M dand at least one non-metal selected from carbon, nitrogen and oxygen. M is at least one metal selected from groups 4a, 5a, 6a (excluding Cr) and Si in the periodic table. a to c are all 15≤a≤40, 55≤b≤75, 10≤c≤20, 0≤d≤15 in atomic ratio, and a+b+c+d=100. As an example, the wear-resistant layer 23 may also be TiAlCrWNbSiN. In addition, d may also be 0. That is, the wear-resistant layer 23 does not necessarily need to contain M. In this case, the wear-resistant layer 23 may also be TiAlCrN, for example.

[0063] The coated tool 1 of the embodiment includes the bonding layer 21 and the wear-resistant layer 23 having the above-mentioned composition, and thus can appropriately suppress boundary wear.

[0064] As factors that contribute to the suppression of boundary damage, film bonding and film resistance to plastic deformation can be cited. Since the bonding layer 21 of the embodiment has a high affinity with the substrate 10 of cemented carbide, the coating layer 20 having the bonding layer 21 at the interface with the substrate 10 has a high bonding with the substrate 10. In addition, the wear-resistant layer 23 having the above composition has a small crystallite diameter, so the coating layer 20 having the wear-resistant layer 23 has a high resistance to plastic deformation.

[0065] Therefore, the coating layer 20 having the bonding layer 21 and the wear-resistant layer 23 can appropriately suppress boundary wear. In particular, the bonding layer 21 of the embodiment is effective in suppressing the secondary boundary wear D2, and the wear-resistant layer 23 of the embodiment is effective in suppressing the primary boundary wear D1.

[0066] The intermediate layer 22 contains Ti e Al f M g and at least one non-metal selected from carbon, nitrogen and oxygen. M is at least one metal selected from groups 4a, 5a, 6a (except Cr) and Si in the periodic table. e and f are 0≤e≤55, 40≤f≤80, and e+f+g=100. The intermediate layer 22 has high oxidation resistance. Therefore, the coated tool 1 having the intermediate layer 22 can appropriately suppress the crater wear D4. As an example, the intermediate layer 22 can also be TiAlWNbSiN. It should be noted that the intermediate layer 22 does not necessarily contain M. In this case, the intermediate layer 22 can also be TiAlN, for example.

[0067] The ratio of the metal components in the intermediate layer 22 can be determined by, for example, EDS (energy dispersive X-ray spectrometer) analysis attached to STEM (scanning transmission electron microscope). Alternatively, the ratio of the metal components in the bonding layer 21 and the wear-resistant layer 23 can also be determined by EDS analysis.

[0068] The intermediate layer 22 may also be formed by arc ion plating (AIP). The AIP method is a method of forming a metal nitride film by evaporating a target metal by arc discharge in a vacuum atmosphere and combining it with N2 gas. At this time, the bias voltage applied to the substrate 10 as the coated object may also be -30V or less. It should be noted that the wear-resistant layer 23 may also be formed by the AIP method.

[0069] It should be noted that, here, an example is shown in which the coating layer 20 is composed of the bonding layer 21, the intermediate layer 22, and the wear-resistant layer 23, but the coating layer 20 does not necessarily need to include the intermediate layer 22. For example, when the object is a cut material that is difficult to produce crater wear D4, the coated tool 1 may also have a coating layer 20 composed of the bonding layer 21 located on the surface of the substrate 10 and the wear-resistant layer 23 located on the surface of the bonding layer 21.

[0070] The thickness of the coating layer 20 may also be 2.5 μm or more and 10 μm or less. When the thickness of the coating layer 20 is 2.5 μm or more, wear resistance (resistance to abrasive wear) is ensured. In addition, when the thickness of the coating layer 20 is 10 μm or less, it is difficult to cause the coating layer 20 to break. Therefore, the coated tool 1 having the coating layer 20 having a film thickness of 2.5 μm or more and 10 μm or less is excellent in wear resistance and breakage resistance.

[0071] The thickness of the bonding layer 21 can also be greater than 2nm and less than 8nm. When the thickness of the bonding layer 21 is greater than 2nm, it is easy to obtain the effect of improving the film bonding brought by the bonding layer 21. In addition, it is difficult to produce uneven film formation, and thus it is difficult to produce abnormal damage. On the other hand, when the thickness of the bonding layer 21 is less than 8nm, the relatively soft bonding layer 21 has less influence on the plastic deformation of the coating layer 20, so it is difficult to produce damage to the coating layer 20. Therefore, the coated tool 1 having a coating layer 20 including a bonding layer 21 having a film thickness of greater than 2nm and less than 8nm can further suppress boundary damage.

[0072] The crystallite diameter of the wear-resistant layer 23 may also be By adopting this structure, the plastic deformation resistance of the coating layer 20 is improved, and the coating layer 20 is difficult to be broken, so that the boundary damage can be further suppressed.

[0073] The crystallite diameter of the wear-resistant layer 23 can be controlled by the composition of the wear-resistant layer 23. The crystallite diameter of the wear-resistant layer 23 can also be controlled by the film forming conditions of the wear-resistant layer 23 (such as bias voltage in physical vapor deposition).

[0074] The Vickers hardness of the wear-resistant layer 23 may also be 28 GPa or more. Secondary boundary wear D2 is generated, for example, by cutting a work-hardened portion with an extremely low cut. Therefore, by setting the hardness of the coating layer 20 to 28 GPa or more, the secondary boundary wear D2 can be appropriately suppressed even when cutting a work material that is prone to work hardening.

[0075] The thickness of the intermediate layer 22 may be smaller than the thickness of the wear-resistant layer 23. When the intermediate layer 22 is made thinner than the wear-resistant layer 23, the effect of suppressing boundary damage by the wear-resistant layer 23 is less likely to decrease. Therefore, by making the thickness of the intermediate layer 22 smaller than the thickness of the wear-resistant layer 23, boundary damage can be appropriately suppressed.

[0076] The coating layer 20 can be arranged on the substrate 10 by using a physical vapor deposition (PVD) method, for example. For example, when the coating layer 20 is formed by the above-mentioned vapor deposition method while the substrate 10 is maintained by the inner circumference of the through hole 5, the coating layer 20 can be arranged in a manner that covers the entire surface of the substrate 10 except the inner circumference of the through hole 5.

[0077] Next, refer to Figure 5 The structure of a cutting tool including the above-mentioned coated tool 1 will be described. Figure 5 This is a front view showing an example of a cutting tool according to an embodiment.

[0078] like Figure 5 As shown, the cutting tool 100 of the embodiment includes a coated tool 1 and a tool holder 70 for fixing the coated tool 1 .

[0079] The handle 70 is from the first end ( Figure 5 ) toward the second end ( Figure 5 The handle 70 is a rod-shaped member extending from the lower end of the handle 70. The handle 70 is made of, for example, steel or cast iron. In particular, when steel is used among these members, the toughness of the handle 70 is high.

[0080] The tool holder 70 has a tool groove 73 at the end of the first end side. The tool groove 73 is a portion for the coated tool 1 to be assembled, and has a seating surface intersecting with the rotation direction of the cut material and a restraining side surface inclined relative to the seating surface. A threaded hole is provided on the seating surface for screwing a screw 75 described later.

[0081] The coated tool 1 is located in the knife groove 73 of the tool holder 70 and is assembled to the tool holder 70 by means of a screw 75. That is, the screw 75 is inserted into the through hole 5 of the coated tool 1, and the front end of the screw 75 is inserted into the threaded hole formed on the seating surface of the knife groove 73 so that the threaded parts are screwed together. Thus, the coated tool 1 is assembled to the tool holder 70 in a manner that the cutting edge portion protrudes outward from the tool holder 70.

[0082] In the embodiment, a cutting tool used in so-called turning processing is illustrated. As turning processing, for example, inner diameter processing, outer diameter processing and slotting processing can be cited. It should be noted that the cutting tool is not limited to the cutting tool used in turning processing. For example, the coated tool 1 can also be used as a cutting tool used in milling processing. As the cutting tool used in milling processing, for example, milling cutters such as flat milling cutters, front milling cutters, side milling cutters, slotting milling cutters, single-edge end mills, multi-edge end mills, tapered edge end mills, ball-end mills, etc. can be cited.

[0083] (Method for producing coating layer)

[0084] Next, an example of a method for producing the coating layer 20 of the present embodiment will be described. It should be noted that the method for producing the coated tool of the present embodiment is not limited to the following method.

[0085] The coating layer may be formed by physical vapor deposition, for example. Examples of the physical vapor deposition method include ion plating and sputtering. As an example, when the coating layer is formed by ion plating, the coating layer may be formed by the following method.

[0086] First, an example of a method for manufacturing a bonding layer is described. As an example, metal targets of Ti, Al, and M (wherein M is at least one metal selected from Groups 4a, 5a, and 6a of the periodic table and Si) or composite alloy targets or sintered targets are prepared.

[0087] Next, the target as a metal source is evaporated and ionized by arc discharge or glow discharge, and the ionized metal is deposited on the surface of the substrate. The bonding layer can be formed by the above procedure.

[0088] The composition of the bonding layer can be adjusted by controlling the voltage and current values ​​of arc discharge and glow discharge applied to various metal targets independently for each target. In addition, the composition of the bonding layer can also be adjusted by controlling the composition of the metal target, the coating time, and the atmospheric pressure. The thickness of the bonding layer can be adjusted, for example, by controlling the coating time.

[0089] Next, a method for manufacturing the wear-resistant layer is described. As an example, metal targets of Ti, Al, Cr, and M (wherein M is at least one metal selected from Groups 4a, 5a, and 6a of the periodic table (excluding Cr) and Si) or composite alloy targets or sintered targets are prepared.

[0090] Next, the target as a metal source is evaporated and ionized by arc discharge or glow discharge, etc. The ionized metal is reacted with nitrogen (N2) gas, etc., and is deposited on the surface of the substrate. The wear-resistant layer can be formed by the above sequence.

[0091] The composition of the wear-resistant layer can be adjusted by controlling the voltage and current value during arc discharge and glow discharge applied to various metal targets independently for each target. In addition, the composition of the wear-resistant layer can also be adjusted by controlling the composition of the metal target, the coating time, and the atmospheric pressure. The thickness of the wear-resistant layer can be adjusted by controlling the coating time, for example.

[0092] Next, an example of a method for manufacturing the intermediate layer is described. As an example, metal targets, composite alloy targets, or sintered targets are prepared from Ti, Al, and M (wherein M is at least one metal selected from Groups 4a, 5a, and 6a of the periodic table (excluding Cr) and Si).

[0093] Next, the target as a metal source is evaporated and ionized by arc discharge or glow discharge, etc. The ionized metal is reacted with nitrogen (N2) gas, etc., and is deposited on the surface of the substrate. The intermediate layer can be formed by the above sequence.

[0094] The composition of the intermediate layer can be adjusted by controlling the voltage and current values ​​during arc discharge and glow discharge applied to various metal targets independently for each target. In addition, the composition of the intermediate layer can also be adjusted by controlling the composition of the metal target, the coating time, and the atmospheric pressure. The thickness of the intermediate layer can be adjusted by controlling the coating time, for example.

[0095] Example

[0096] Hereinafter, examples of the present invention will be described in detail. It should be noted that the present invention is not limited to the examples shown below.

[0097] (X-ray intensity distribution of the coating layer with respect to the positive pole figure of the (111) plane)

[0098] For a material having a composition of TiAlNbWSi, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 The bonding layer is composed of TiAlWNbSiN, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 N and an intermediate layer composed of TiAlCrWNbSiN, specifically Al59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 For the coated cutting tool with a wear-resistant layer composed of N, the X-ray intensity distribution was measured. The measurement conditions are as follows. It should be noted that when the normal of the sample surface is in the plane determined by the incident ray and the diffracted ray, the angle of the α-axis is set to 90°. When the angle of the α-axis is 90°, it becomes the center point on the pole figure.

[0099] <Measurement Conditions of X-ray Intensity Distribution>

[0100] (1) Flat collimator

[0101] (2) Scanning method: Concentric circles

[0102] (3) β-scanning range: 0° or more and 360° or less / 2.5° interval

[0103] (4) θ fixed angle: The angle at which the diffraction intensity is the highest during the period from 37° to 39° for the (111) plane diffraction angle of the TiAlN crystal contained in the coating layer (wear-resistant layer). The angle at which the diffraction intensity is the highest during the period from 43° to 45° for the (200) plane diffraction angle of the TiAlN crystal contained in the coating layer (wear-resistant layer).

[0104] (5) α-scanning range: 0° or more and 90° or less / 2.5° step

[0105] (6) Target: CuKα, Voltage: 45 kV, Current: 40 mA

[0106] Figure 6 It is a chart showing the X-ray intensity distribution of the pole figure of the cubic crystal contained in the coating layer with respect to the (iii) plane. Figure 6 The horizontal axis of the pole figure shown represents the angle of the α-axis (tilt axis), and the vertical axis represents the X-ray intensity in the tilt direction.

[0107] The orientation of the (iii) plane in the cubic crystal can be evaluated by the X-ray intensity distribution of the pole figure with respect to the (iii) plane. For example, the X-ray intensity distribution with a peak at the 35° position in the X-ray intensity distribution of the pole figure with respect to the (iii) plane indicates that there are more cubic crystals with the (iii) plane tilted 35° relative to the surface of the substrate.

[0108] As Figure 6As shown, the X-ray intensity distribution of the α-axis of the positive pole diagram of the cubic crystal contained in the coating layer (wear-resistant layer) with respect to the (iii) plane is flat within the range of the α-axis angle being greater than 30° and less than 90°. Specifically, the maximum value (Imax) of the X-axis intensity within the range of the α-axis angle being greater than 30° and less than 90° is 1064 (α-axis angle = 70°), and the minimum value (Imin) is 990 (α-axis angle = 30°). Furthermore, the difference between the maximum value (Imax) and the minimum value (Imin) is 74, which is less than 10% of 1064, which is the maximum value (Imax). Specifically, the difference between the maximum value (Imax) and the minimum value (Imin) is less than 7% of the maximum value (Imax).

[0109] Thus, in the measurement range of the coating layer of the embodiment, in the X-ray intensity distribution of the α-axis of the positive pole diagram of the (111) plane of the cubic crystal, the difference between the maximum value (Imax) and the minimum value (Imin) of the X-ray intensity in the range of 30° to 90° is less than 10% of the maximum value (Imax). According to this result, it can be seen that the coating layer of the embodiment has a homogeneous structure with a certain degree of uniform crystal orientation. Thus, the coating layer of the embodiment can suppress abnormal wear such as collapse, for example.

[0110] (X-ray intensity distribution of the coating layer with respect to the positive pole figure of the (200) plane)

[0111] Figure 7 This is a graph showing the X-ray intensity distribution of the positive pole figure of the cubic crystal contained in the coating layer with respect to the (200) plane. Figure 7 In the positive pole diagram shown, the horizontal axis represents the angle of the α-axis (inclined axis), and the vertical axis represents the X-ray intensity in the inclined direction.

[0112] like Figure 7 As shown, the coating layer of the embodiment has a maximum value and a minimum value of X-ray intensity in the measurement range of 0° to 90° in the X-ray intensity distribution of the α-axis of the positive pole diagram of the (200) plane of the cubic crystal, and in the range of 0° to 50° of the angle of the α-axis. Specifically, the coating layer of the embodiment has a maximum value (Ilmax) at a position of 25° on the α-axis, and its value is 939. In addition, the coating layer of the embodiment has a minimum value (Ilmin) at a position of 40° on the α-axis, and its value is 849. Furthermore, the difference between the maximum value (Ilmax) and the minimum value (Ilmin) is 90, which is less than 10% of 930, which is the maximum value (Ilmax).

[0113] Thus, the coating layer of the embodiment has a maximum value and a minimum value of X-ray intensity in the measurement range of 0° and below 90° in the X-ray intensity distribution of the α-axis of the positive pole diagram of the (200) plane of the cubic crystal, and in the range of 0° and below 50° of the angle of the α-axis. In addition, the difference between the above-mentioned maximum value and the above-mentioned minimum value of the coating layer of the embodiment is less than 10% relative to the maximum value. According to this result, it can be seen that the coating layer of the embodiment has a homogeneous structure with a certain degree of consistent crystal orientation. Therefore, the coating layer of the embodiment can, for example, suppress abnormal wear such as collapse.

[0114] (Composition of wear-resistant layer)

[0115] For those with Ti a Al b Cr c M d The wear-resistant layer has a composition of Ti x Al y M z The bonding layer has a composition of Ti e Al f M g The coating layer of the intermediate layer with the composition of Al was prepared to produce multiple samples (samples No. 1 to No. 15) with different composition ratios (a to d) of the wear-resistant layer. The composition ratios (a to d) of the wear-resistant layer and the composition of M in samples No. 1 to No. 15 are shown in Table 1. The composition of the bonding layer in samples No. 1 to No. 15 is Al 49 Ti 46 M 5 , specifically Al 49 Ti 46 W 2 Nb 2 Si 1 In addition, the composition of the intermediate layer in samples No. 1 to No. 15 is Al 49 Ti 46 M 5 N, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 N. The film thicknesses of the wear-resistant layer, the bonding layer, and the intermediate layer in samples No. 1 to No. 15 were 4.5 μm, 5 nm, and 2 μm, respectively.

[0116] For the prepared samples No. 1 to No. 15, the crystallite diameter of the (200) surface, the hardness of the wear-resistant layer, the primary boundary wear amount, and the secondary boundary wear amount were measured. The crystallite diameter of the (200) surface was measured using XRD. The hardness (Vickers hardness) of the wear-resistant layer was measured using a micro-indentation hardness tester "ENT-1100b / a" (manufactured by Elionix Co., Ltd.). For each sample, the depth from the surface of the wear-resistant layer (i.e., the surface of the coating layer) to 20% of the thickness of the wear-resistant layer was used as the measurement range, and the hardness was measured under the indentation load of 30N. The measurement of the primary boundary wear amount and the secondary boundary wear amount was measured based on the images obtained by photographing the primary boundary and the secondary boundary of each sample after the cutting test under the following conditions.

[0117] <Cutting test conditions>

[0118] Cutting material: Inconel (registered trademark) 718

[0119] Cutting speed (Vc): 30m / min

[0120] Feed (f): 0.1mm / rev

[0121] Cutting depth (ap): 0.5mm

[0122] Cutting state: wet

[0123] Tool used: CNMG120408SG

[0124] Cutting time: 7.4min

[0125] [Table 1]

[0126]

[0127] Figure 8 This is a graph showing the correlation between the crystallite diameter in the (200) plane of the wear-resistant layer and the primary boundary wear amount. Figure 8 The horizontal axis of the graph shown is the crystallite diameter of the (200) plane. The vertical axis is the secondary boundary wear amount (mm).

[0128] like Figure 8 As shown in FIG. 1 , it can be observed that the smaller the crystallite diameter of the (200) surface in the wear-resistant layer is, the smaller the primary boundary wear amount is. Based on this result, it can be seen that the crystallite diameter of the wear-resistant layer is preferably smaller. Specifically, the crystallite diameter of the wear-resistant layer is preferably That is, the crystallite diameter of the (200) plane in samples No. 1 to No. 15 is The following samples No. 1 to No. 7 and No. 13 are effective in suppressing primary boundary damage.

[0129] Fig. 9 This is a graph showing the correlation between the Vickers hardness of the wear-resistant layer and the secondary boundary wear amount. Fig. 9 In the graph shown, the horizontal axis represents the Vickers hardness (GPa) of the wear-resistant layer, and the vertical axis represents the secondary boundary wear amount (mm).

[0130] like Fig. 9 As shown in the figure, it can be observed that the higher the Vickers hardness of the wear-resistant layer, the greater the secondary boundary wear amount. It can be seen that when the Vickers hardness of the wear-resistant layer is 28 GPa or more, the secondary boundary wear amount is appropriately suppressed. That is, it can be seen that among samples No. 1 to No. 15, samples No. 1, No. 3, No. 5 to No. 9 with a Vickers hardness of 28 GPa or more are effective in suppressing secondary boundary damage.

[0131] Fig.10 This is a graph showing the correlation between the Ti ratio (a) of the wear resistant layer and the primary boundary wear amount. Fig.10 In the graph shown, the horizontal axis represents the Ti ratio of the wear-resistant layer, and the vertical axis represents the primary boundary wear amount (mm).

[0132] according to Fig.10 The results shown show that the samples with a Ti ratio (a) of 15 ≤ a ≤ 40, specifically samples No. 1 to No. 9, No. 11 to No. 13, are effective in suppressing primary boundary damage. In addition, the samples with a Ti ratio (a) of 20 ≤ a ≤ 30, specifically samples No. 1 to No. 6, No. 8, No. 9, No. 11 to No. 13, are particularly effective in suppressing primary boundary damage.

[0133] Fig.11 This is a graph showing the correlation between the A1 ratio (b) of the wear-resistant layer and the primary boundary wear amount. Fig.11 In the graph shown, the horizontal axis represents the A1 ratio of the wear-resistant layer, and the vertical axis represents the primary boundary wear amount (mm).

[0134] according to Fig.11 The results shown show that the samples with an A1 ratio (b) of 55≤b≤75, specifically samples No. 1, No. 3 to No. 13, are effective in suppressing primary boundary damage. In addition, the samples with an A1 ratio (b) of 55≤b≤70, specifically samples No. 1, No. 3 to No. 8, No. 10 to No. 12, are particularly effective in suppressing primary boundary damage.

[0135] Fig.12 This is a graph showing the correlation between the Cr ratio (c) of the wear-resistant layer and the primary boundary wear amount. Fig.12 In the graph shown, the horizontal axis represents the Cr ratio of the wear-resistant layer, and the vertical axis represents the primary boundary wear amount (mm).

[0136] according to Fig.12 The results shown show that the samples with a Cr ratio (c) of 5 ≤ c ≤ 20, specifically samples No. 1 to No. 12, are effective in suppressing primary boundary damage. In addition, the samples with a Cr ratio (c) of 10 ≤ c ≤ 20, specifically samples No. 1 to No. 7 and No. 9, are particularly effective in suppressing primary boundary damage.

[0137] In order to effectively suppress secondary boundary damage in addition to primary boundary damage, Ti a Al b Cr c M d The composition ratio (a-d) of the wear-resistant layer is preferably within the range of 15≤a≤40, 55≤b≤75, 10≤c≤20, 0≤d≤15 (where a+b+c+d=100). More specifically, the composition ratio (a-d) of the wear-resistant layer is preferably 20≤a≤30, 55≤b≤70, 15≤c≤20, 2.5≤d≤15.

[0138] (Composition of the bonding layer)

[0139] For those with Ti a Al b Cr c M d The wear-resistant layer has a composition of Ti x Al y M z The bonding layer has a composition of Ti e Al f M g The composition ratios (x to z) of the bonding layer and the composition of M in the bonding layer of samples No. 21 to No. 38 are shown in Table 2. The composition of the wear-resistant layer in samples No. 21 to No. 38 is A1 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N. The composition of the intermediate layer in samples No. 21 to No. 38 is Al 49 Ti 46 M 5 N, specifically Al 49 Ti 46 W 2 Nb2 Si 1 N. The film thicknesses of the wear-resistant layer, the bonding layer, and the intermediate layer in samples No. 21 to No. 38 were 4.5 μm, 5 nm, and 2 μm, respectively.

[0140] For the samples No. 21 to No. 38 produced, the thickness of the bonding layer, the peeling load, the primary boundary wear amount and the secondary boundary wear amount were measured. The thickness of the bonding layer was measured based on the image obtained by observing the bonding layer using a transmission electron microscope (TEM). Specifically, the average value of the measurement results of 9 points in each of the three fields of view was taken as the thickness of the bonding layer. The peeling load was measured by a scratch test. The scratch test was carried out under the conditions of a scratching speed of 10 mm / min and a load addition speed of 100 N / min using a diamond indenter with a front end shape of R (radius of curvature) of 200 μm. In the scratch test, the load (peeling load) when peeling was generated was evaluated as the bonding force. In the scratch test, the larger the critical load, the more difficult it is to peel, that is, the higher the bonding force. The measurement of primary boundary wear and secondary boundary wear is the same as that of the above-mentioned samples No. 1 to No. 15. These measurement results are also shown in Table 2.

[0141] [Table 2]

[0142]

[0143] Fig.13 This is a graph showing the correlation between the peeling load and the secondary boundary wear amount. Fig.13 In the graph shown, the horizontal axis represents the peeling load (N) and the vertical axis represents the secondary boundary wear amount (mm).

[0144] like Fig.13 As shown, it can be seen that the higher the peeling load, that is, the higher the bonding force, the smaller the secondary boundary wear amount, that is, the more the secondary boundary damage is suppressed.

[0145] Fig.14 : is a graph showing the correlation between the Ti ratio (x) of the bonding layer and the peeling load. Fig.15 : is a graph showing the correlation between the Al ratio (y) of the tie layer and the peeling load. Fig.16 Graph showing the correlation between the Ti ratio (x) of the bonding layer and the secondary boundary wear amount. Fig.17 It is a graph showing the correlation between the Al ratio (y) of the bonding layer and the secondary boundary wear amount.

[0146] according to Fig.13 The results and Figure 14 to Figure 17As a result, in order to effectively suppress secondary boundary damage, it is preferred that the Ti ratio of the bonding layer is relatively high and the Al ratio is relatively low. Specifically, the composition ratio (x-z) of the bonding layer is preferably within the range of 40≤x≤80, 0≤y≤55 (where x+y+z=100).

[0147] (Composition of the middle layer)

[0148] For those with Ti a Al b Cr c M d The wear-resistant layer has a composition of Ti x Al y M z The bonding layer has a composition of Ti e Al f M g The composition of the intermediate layer of the coating layer is Al, and multiple samples (samples No. 41 to No. 49) with different composition ratios (e to g) of the intermediate layer are prepared. The composition ratios (e to g) of the intermediate layer and the composition of M in samples No. 41 to No. 49 are shown in Table 3. The composition of the wear-resistant layer is Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N. The composition of the bonding layer is Al 49 Ti 46 M 5 , specifically Al 49 Ti 46 W 2 Nb 2 Si 1 The film thicknesses of the wear-resistant layer, the bonding layer, and the intermediate layer in samples No. 41 to No. 49 were 2.5 μm, 5 nm, and 2 μm, respectively.

[0149] In addition, the crater wear depth was measured for the prepared samples No. 41 to No. 49. The crater wear depth was measured based on the images obtained by photographing the rake face of each sample after the cutting test was carried out under the same conditions as the measurement of the primary boundary wear amount and the secondary boundary wear amount of the wear-resistant layer and the bonding layer. The measurement results are also shown in Table 3.

[0150] [Table 3]

[0151] (Table 3)

[0152]

[0153] Fig.18This is a graph showing the correlation between the Ti ratio (e) of the intermediate layer and the crater wear depth. Fig.18 The horizontal axis of the graph shown is the Ti ratio of the intermediate layer, and the vertical axis is the crater wear depth (mm). Fig.19 This is a graph showing the correlation between the Al ratio (f) of the intermediate layer and the crater wear depth. Fig.19 In the graph shown, the horizontal axis represents the Al ratio of the intermediate layer, and the vertical axis represents the crater wear depth (mm).

[0154] according to Fig.18 as well as Fig.19 The results show that in order to effectively suppress crater wear, the composition ratio (e to g) of the intermediate layer is preferably within the range of 0≤e≤55 and 40≤f≤80 (where e+f+g=100).

[0155] (Comparison of boundary wear caused by differences in film structure)

[0156] Coated tools having a coating layer consisting of a bonding layer and a single-layer wear-resistant layer on the surface of the substrate (the above-mentioned samples No. 3, No. 24, and No. 43. It should be noted that samples No. 3, No. 24, and No. 43 are the same samples), coated tools having a coating layer consisting of only a single-layer wear-resistant layer on the surface of the substrate, and coated tools having a wear-resistant layer consisting of two layers of different compositions alternately stacked on the surface of the substrate were produced. The substrate includes a hard phase containing WC and a metal bonding phase containing an iron group element. The composition of the bonding layer is Al 49 Ti 46 W 2 Nb 2 Si 1 The composition of the single-layer wear-resistant layer is Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N. The compositions of each layer in the wear-resistant layer formed by alternately stacking two layers are AlCrN and AlTiWNbSiN, respectively.

[0157] The cutting test was carried out using the three prepared samples under the following conditions.

[0158] <Cutting test conditions>

[0159] Cutting material: Inconel (registered trademark) 718

[0160] Cutting speed (Vc): 30m / min

[0161] Feed (f): 0.1mm / rev

[0162] Cutting depth (ap): 0.5mm

[0163] Cutting state: wet

[0164] Tool used: CNMG120408SG

[0165] The state of the tool tip after cutting for 14.8 minutes under the above cutting conditions was Fig. 20 Shown in. Fig. 20 The images show the state of the cutting edge of three coated cutting tools having different film structures after the cutting test.

[0166] like Fig. 20 As shown in the figure, the coated tool having the film structure of "a bonding layer and a single-layer wear-resistant layer" has reduced primary boundary wear and secondary boundary wear compared to the coated tool having the film structure of "only a single-layer wear-resistant layer" and the coated tool having the film structure of "a wear-resistant layer formed by alternating two layers". Based on this result, it can be seen that the film structure of "a bonding layer and a single-layer wear-resistant layer" is effective in suppressing boundary wear.

[0167] In addition, the coated tool with the film structure of "a bonding layer and a single-layer wear-resistant layer" also has reduced abrasive wear compared to the coated tool with the film structure of "only a single-layer wear-resistant layer" and the coated tool with the film structure of "a wear-resistant layer formed by alternating two layers". Based on this result, it can be seen that the film structure of "a bonding layer and a single-layer wear-resistant layer" is also effective in suppressing abrasive wear.

[0168] (Composition of the bonding layer)

[0169] For coated tools with a film structure of "bonding layer and single-layer wear-resistant layer", multiple samples with different bonding layer compositions were prepared. The bonding layer compositions were Ti, Cr, Al, TiCr, AlCr, TiAl, TiAlCr and TiAlNbWSi. TiAlNbWSi is specifically Al 49 Ti 46 W 2 Nb 2 Si 1 Furthermore, cutting tests were conducted on the prepared samples under the same conditions as above. It should be noted that the composition of the wear-resistant layer was TiAlNbWSiN, specifically Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N.

[0170] The state of the tool tip after 7.4 minutes of cutting under the above cutting conditions was Fig.21 Shown in. Fig.21 The images show the state of the cutting edge of eight coated cutting tools having different bonding layer compositions after the cutting test.

[0171] like Fig.21 As shown, changes are shown in the wear state according to the composition of the bonding layer. Specifically, it is known that the coated tool having a bonding layer composed of TiAl and the coated tool having a bonding layer composed of TiAlNbWSi have suppressed primary boundary wear, secondary boundary wear and abrasive wear compared to the coated tool having a bonding layer of other compositions.

[0172] (Composition of wear-resistant layer)

[0173] For coated tools with a film structure of "bonding layer and single-layer wear-resistant layer", multiple samples with different compositions of the wear-resistant layer were prepared. The compositions of the wear-resistant layer were TiAlN, TiAlSiN, TiAlNbN, TiAlWN, TiAlCrN, TiAlWNbSiN and TiAlCrWNbSiN. TiAlCrWNbSiN is specifically Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N, and cutting tests were conducted on the prepared samples under the same conditions as above. It should be noted that the composition of the bonding layer was TiAlNbWSi, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 .

[0174] The state of the tool tip after 7.4 minutes of cutting under the above cutting conditions was Fig. 22 Shown in. Fig. 22 The images show the state of the cutting edge of seven coated cutting tools having different compositions of the wear-resistant layer after the cutting test.

[0175] like Fig. 22 Specifically, it is found that the coated tool having a wear-resistant layer composed of TiAlCrWNbSiN has suppressed primary boundary wear, secondary boundary wear, and abrasive wear compared to coated tools having wear-resistant layers of other compositions.

[0176] (Thickness of wear-resistant layer)

[0177] For a material having a composition of TiAlNbWSi, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 The bonding layer is composed of TiAlCrWNbSiN, specifically Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N-composition wear-resistant layer coated tools, multiple samples with different wear-resistant layer thickness were produced. The coating layer thickness of each sample was 1.7μm, 3.1μm, 3.4μm, 4.1μm, 4.7μm, 5.3μm and 5.8μm respectively. The thickness of the bonding layer is the same in any sample. Therefore, the thicker the coating layer, the thicker the wear-resistant layer. The average thickness of the bonding layer is 5nm℃

[0178] Cutting tests were conducted on the prepared samples under the same conditions as above. Furthermore, the length of abrasive wear in the thickness direction of the coating layer of each sample was measured using images showing the blade tip state of each sample after the test (hereinafter referred to as "abrasive wear amount"). It should be noted that the cutting time in the cutting test was 15 minutes.

[0179] Fig.23 This is a graph showing the relationship between the film thickness of the wear-resistant layer and the amount of abrasive wear. Fig.23 The horizontal axis of the graph shown is the total film thickness of the coating layer, that is, the total of the film thickness of the bonding layer and the film thickness of the wear-resistant layer. Fig.23 The vertical axis of the graph shown is the abrasive wear amount.

[0180] It should be noted that a cutting test was conducted on a commercially available coated tool having a coating layer thickness of 5 μm under the same cutting conditions as above, and then the abrasive wear amount was measured. Fig.23 Indicated by the black circle mark.

[0181] like Fig.23 As shown in FIG. 1 , the thicker the wear-resistant layer, the less abrasive wear there is. For example, in order to suppress the abrasive wear to less than 1 mm, the thickness of the coating layer is preferably 2.5 μm or more. In addition, by setting the total thickness of the coating layer to about 3 μm, the abrasive wear is the same as that of the commercial product. In addition, according to Fig.23As a result, in order to reduce the abrasive wear as much as possible, it is preferred that the total film thickness of the coating layer is set to be 4.1 μm or more. On the other hand, when the film thickness of the coating layer is thicker than 10 μm, film formation becomes difficult. Therefore, the thickness of the coating layer is preferably 2.5 μm or more and 10 μm or less, more preferably 4.1 μm or more and 10 μm or less.

[0182] (Thickness of bonding layer)

[0183] For a material having a composition of TiAlNbWSi, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 The bonding layer is composed of TiAlCrWNbSiN, specifically Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 A coated tool with a wear-resistant layer composed of N was used to produce multiple samples with different film thicknesses of the bonding layer. The film thickness of the bonding layer can be controlled by adjusting the film forming time of the bonding layer, so that the longer the film forming time, the thicker the film thickness of the bonding layer. The film forming time of the bonding layer of each sample is 0min, 0.7min, 1.5min and 3min respectively. In addition, the film thickness of the bonding layer of each sample is 0nm, 1nm, 5nm and 10nm respectively.

[0184] Cutting tests were conducted on the prepared samples under the same conditions as above. Furthermore, the length of primary boundary wear (hereinafter referred to as "primary boundary wear amount"), the length of secondary boundary wear (hereinafter referred to as "secondary boundary wear amount"), and the length of abrasive wear (hereinafter referred to as "abrasive wear amount") in the thickness direction of the coating layer of each sample were measured using images showing the blade edge state of each sample after the test. The cutting time in the cutting test was 7.4 minutes.

[0185] Fig.24 is a graph showing the relationship between the film formation time of the bonding layer and various wear amounts. Fig.24 As shown in FIG. 1 , it can be observed that the longer the bonding layer is formed, that is, the thicker the bonding layer is, the lower the wear amount is. This tendency is particularly significant in the case of secondary boundary wear. Fig.24 The results shown show that in order to suppress all of the primary boundary wear, the secondary boundary wear, and the side wear, the thickness of the bonding layer is preferably 2 nm or more and 8 nm or less.

[0186] In addition, for Fig.24The same samples as those shown above, that is, samples with the film forming time of the bonding layer set to 0 min, 0.7 min, 1.5 min, and 3 min, were subjected to a defect resistance test. The conditions were as follows.

[0187] <Defect Resistance Test>

[0188] Cutting material: SUS304

[0189] Cutting speed: 150m / min

[0190] Feed: 0.2mm / rev

[0191] Cutting depth: 1mm

[0192] Cutting state: wet

[0193] Tool used: CNMG120408SG

[0194] Evaluation method: Number of impacts until failure (times)

[0195] Fig.25 is a graph showing the relationship between the film formation time of the bonding layer and the number of impacts until the defect. Fig.25 As shown in FIG. 1 , it is known that when the film forming time exceeds 1.5 min, the defect resistance decreases. Fig.24 as well as Fig.25 The results shown show that the thickness of the bonding layer is preferably 2 nm or more and 8 nm or less. It should be noted that the thickness of the bonding layer can be derived from the film formation time.

[0196] (Middle layer)

[0197] For a material having a composition of TiAlNbWSi, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 The bonding layer is composed of TiAlCrWNbSiN, specifically Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5 N-based coated tools with a wear-resistant layer, samples with an intermediate layer between the bonding layer and the wear-resistant layer and samples without an intermediate layer were produced. The composition of the intermediate layer is TiAlWNbSiN, specifically Al 49 Ti 46 W 2 Nb 2 Si 1N. Furthermore, a cutting test was performed on the produced samples under the following conditions.

[0198] <Cutting test conditions>

[0199] Cutting material: SUS304

[0200] Cutting speed: 150m / min

[0201] Feed: 0.2mm / rev

[0202] Cutting depth: 1mm

[0203] Cutting state: wet

[0204] Tool used: CNMG120408SG

[0205] The state of the tool tip after 39 minutes of cutting under the above cutting conditions was Fig.26 as well as Fig. 27 Shown in. Fig.26 This is an image obtained by photographing the state of the cutting edge of a sample having an intermediate layer after a cutting test from a direction perpendicular to the rake face. Fig. 27 This is an image obtained by photographing the state of the cutting edge of a sample having no intermediate layer after a cutting test from a direction perpendicular to the rake face.

[0206] according to Fig.26 as well as Fig. 27 As is clear from the images shown, by interposing the intermediate layer between the bonding layer and the wear-resistant layer, the crater wear generated on the rake face is appropriately suppressed.

[0207] (Thickness ratio of the intermediate layer to the wear-resistant layer)

[0208] For a material having a composition of TiAlNbWSi, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 The bonding layer is composed of TiAlWNbSiN, specifically Al 49 Ti 46 W 2 Nb 2 Si 1 N and an intermediate layer composed of TiAlCrWNbSiN, specifically Al 59.5 Ti 23 Cr 15 W 1 Nb 1 Si 0.5A plurality of samples with different film thickness ratios of the intermediate layer and the wear-resistant layer were prepared for a coated tool having a wear-resistant layer composed of N. In addition, a coated tool without an intermediate layer and a coated tool without a wear-resistant layer were prepared. A cutting test was performed on each of the prepared samples under the following conditions, and the state of the tool tip after the cutting test was observed. The cutting time was 14.8 minutes.

[0209] <Cutting test conditions>

[0210] Cutting material: Inconel (registered trademark) 718

[0211] Cutting speed (Vc): 30m / min

[0212] Feed (f): 0.1mm / rev

[0213] Cutting depth (ap): 0.5mm

[0214] Cutting state: wet

[0215] Tool used: CNMG120408SG

[0216] Fig.28 This is a table that summarizes the film thicknesses of the intermediate layer and the wear-resistant layer of five samples having different film thickness ratios of the intermediate layer and the wear-resistant layer, and images showing the state of the cutting edge after the cutting test.

[0217] like Fig.28 As shown, sample No. 51 is a sample without an intermediate layer. Specifically, the film thickness of the wear-resistant layer of sample No. 51 is 4 μm, and the film thickness of the intermediate layer is 0 μm. The film thickness of the wear-resistant layer of sample No. 52 is 2.5 μm, and the film thickness of the intermediate layer is 1.5 μm. The film thickness of the wear-resistant layer and the intermediate layer of sample No. 53 are both 2 μm. The film thickness of the wear-resistant layer of sample No. 54 is 1.5 μm, and the film thickness of the intermediate layer is 2.5 μm. Sample No. 55 is a sample without a wear-resistant layer. Specifically, the film thickness of the wear-resistant layer of sample No. 55 is 0 μm, and the film thickness of the intermediate layer is 4 μm.

[0218] like Fig.28 As shown, samples No. 54 and No. 55, where the intermediate layer is thicker than the wear-resistant layer, have larger boundary damage than samples No. 51 to No. 53, where the intermediate layer is thinner than the wear-resistant layer. Based on this result, the thickness of the intermediate layer is preferably less than the thickness of the wear-resistant layer.

[0219] It should be noted that Figure 1The shape of the coated tool 1 shown is only an example and does not limit the shape of the coated tool according to the present invention. The coated tool according to the present invention may also have, for example: a rod-shaped body having a rotation axis and extending from a first end to a second end; a cutting edge located at the first end of the body; and a groove extending spirally from the cutting edge toward the second end side of the body.

[0220] Further effects and variations can be easily derived by those skilled in the art. Therefore, the broader scheme of the present invention is not limited to the specific detailed and representative embodiments shown and described above. Therefore, various changes can be made without departing from the spirit or scope of the concept of the general invention defined by the attached technical solutions and their equivalents.

[0221] Description of Reference Numerals

[0222] 1 Coated tool

[0223] 2 Blade body

[0224] 4a Periodic Table

[0225] 5Through holes

[0226] 10 Matrix

[0227] 20 coating layers

[0228] 21 Binding layer

[0229] 22 Middle layer

[0230] 23 Wear-resistant layer

[0231] 100 cutting tools

[0232] 201 Corner

[0233] D1 primary boundary wear

[0234] D2 Secondary Boundary Wear

[0235] D3 Abrasive Wear

[0236] D4 crater wear.

Claims

1. A coated tool, wherein: The coated tool comprises a substrate and a coating layer located on the surface of the substrate. The coating layer contains cubic crystals composed of at least one element selected from the periodic table 4a, 5a, 6a group elements, Al, Si, B, Y and Mn, and at least one element selected from C and N. In the measurement range of greater than 0° and less than 90° in the X-ray intensity distribution of the α-axis of the positive pole diagram of the (111) plane of the coating layer, the difference between the maximum and minimum values ​​of the X-ray intensity in the range of greater than 30° and less than 90° of the α-axis is less than 10% of the maximum value.

2. A coated tool, wherein: The coated tool comprises a substrate and a coating layer located on the surface of the substrate. The coating layer contains cubic crystals composed of at least one element selected from the periodic table 4a, 5a, 6a group elements, Al, Si, B, Y and Mn, and at least one element selected from C and N. In the measurement range of above 0° and below 90° in the X-ray intensity distribution of the α-axis of the positive pole diagram of the (200) plane of the coating layer, there is a maximum value and a minimum value of the X-ray intensity in the range of the angle of the α-axis being above 0° and below 50°, and the difference between the maximum value and the minimum value is less than 10% of the maximum value.

3. The coated tool according to claim 1 or 2, wherein: The coating layer has a thickness of 2.5 μm or more and 10 μm or less.

4. The coated tool according to any one of claims 1 to 3, wherein: The crystallite diameter of the coating layer is the following.

5. The coated tool according to any one of claims 1 to 4, wherein: The coating layer includes a bonding layer in contact with the substrate and a wear-resistant layer. The Vickers hardness of the wear-resistant layer is greater than 28 GPa.

6. The coated tool according to claim 1 or 2, wherein: The coating layer includes a bonding layer in contact with the substrate and a wear-resistant layer. The thickness of the bonding layer is greater than or equal to 2 nm and less than or equal to 8 nm.

7. The coated tool according to any one of claims 1 to 6, wherein: The coating layer includes a bonding layer in contact with the substrate, an intermediate layer in contact with the bonding layer, and an anti-wear layer in contact with the intermediate layer. The intermediate layer includes Ti e Al f M g and at least one non-metal selected from carbon, nitrogen and oxygen, M is at least one metal selected from Groups 4a, 5a, 6a of the periodic table other than Cr and Si, all of which are 0≤e≤55, 40≤f≤80 in atomic ratio, wherein e+f+g=100.

8. A cutting tool, wherein: The cutting tool has: A rod-shaped handle having a knife groove at the end; and The coated cutting tool according to any one of claims 1 to 7, which is located in the cutting groove.