Method for producing crystalline sodium sulfate
By combining aqueous sulfate solutions containing nickel and cobalt and manganese with sodium hydroxide or sodium carbonate in the presence of ammonia or ammonia, and filtration, distillation and porous membrane permeation, the purity and odor of sodium sulfate in the prior art are solved. Problem, obtaining high-purity sodium sulfate suitable for builders and reducing production costs.
Patent Information
- Application Number
- CN202380028839.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to produce sodium sulfate that satisfies purity, odorless and colorless from cheap sources, and is suitable as a builder for clothing detergents.
By combining a aqueous sulfate solution containing nickel and cobalt, manganese with sodium hydroxide or sodium carbonate aqueous solution in the presence of ammonia or ammonia salt, filtering, distillation, porous membrane permeation and evaporation treatment after precipitation, impurities and water are removed, and high-quality water is obtained by combining a aqueous solution containing nickel and cobalt and manganese. Sodium sulfate of purity.
High purity, colorless and odorless sodium sulfate production is achieved, suitable as a builder, and reduces production costs.
Abstract
Description
[0001] The present invention relates to a method for producing crystalline sodium sulfate, the method comprising the following steps:
[0002] (a) combining an aqueous solution containing nickel and a sulfate salt of at least one metal selected from cobalt and manganese with an aqueous solution of sodium hydroxide or sodium carbonate in a stoichiometric ratio of about 1:2 or 1:1, respectively, in the presence of ammonia or an ammonia salt,
[0003] (b) removing the precipitated nickel and at least one hydroxide or carbonate of a metal selected from the group consisting of cobalt and manganese by filtration,
[0004] (c) removing ammonia from the filtrate from step (b) by stripping in a distillation column,
[0005] (d) passing the remaining liquid phase through the porous membrane, thereby obtaining a permeate, and
[0006] (e) removing water from the permeate from step (d) by evaporation.
[0007] Alkali metal sulfates such as sodium sulfate are useful products in many applications, for example, they can be used as builders in laundry detergents. However, in order to be suitable builders, such sulfates need to meet several criteria. They must not contain key impurities. They must be colorless and should not impart an unpleasant odor to the laundry detergent. Furthermore, they must not be a cost factor for the laundry detergent.
[0008] Large amounts of sodium sulfate are obtained from mineral resources, for example from Glauber's salt. However, alternative processes are also of interest.
[0009] In CN 112299638 A1, a process for obtaining sodium sulfate from the filtrate of a ternary precursor precipitated from sulfate and sodium hydroxide is described. The obtained sodium sulfate may still not be suitable for builder or other home care applications.
[0010] In WO 2019 / 117411, a method for post-treatment of filtrates is described, in which ammonia, a complexing agent commonly used in precursor production, is recovered in the form of ammonium sulfate.
[0011] In US 6,001,246 a process is disclosed in which sodium sulfate is produced from wastewater. The sodium sulfate contains about 0.200% by weight of NaCl.
[0012] The object of the present invention is to provide a process for producing sodium sulfate from an inexpensive source which meets the above-mentioned requirements of purity, odorlessness and colorlessness, without having the disadvantages of the prior art processes. A further object of the present invention is to provide an apparatus in which a corresponding process can be carried out.
[0013] Accordingly, a method as defined at the outset has been found, which is also referred to hereinafter as the inventive method. The inventive method comprises steps (a) to (e), which are also referred to hereinafter as step (a) or simply (a), step (b) or simply (b), etc. The inventive method will be described in more detail below.
[0014] Step (a) comprises combining an aqueous solution containing nickel and a sulfate salt of at least one metal selected from cobalt and manganese with an aqueous solution of sodium hydroxide or sodium carbonate in a stoichiometric ratio of about 1:2 or 1:1, respectively, in the presence of ammonia or an ammonia salt.
[0015] The relative amount of nickel and at least one metal selected from cobalt and manganese can be selected in a wide range. Nickel can account for 25 to 97mol-% of the metal except alkali metal. Cobalt may not exist, or exist and can account for 1 to 33mol-%, preferably 2 to 20mol-% of the metal except alkali metal. Manganese may not exist, or exist and can account for 1 to 75mol-%, preferably 2 to 68mol-% of the metal except alkali metal. The other metal that can be present in step (a) is magnesium or aluminum, for example up to 2mol-% magnesium or up to 10mol-% aluminum. When aluminum is present in an amount of 3 to 10mol-%, cobalt is preferably also present.
[0016] During step (a), precipitation is carried out.
[0017] In one embodiment of the present invention, by introducing MgSO 4 、Al 2 (SO 4 ) 3 、NaAl(OH) 4 、NaAl(SO 4 ) 2 and KAl(SO 4 ) 2 At least one of aluminum and magnesium is included in the precipitation in step (a).
[0018] Sodium hydroxide is able to absorb carbon dioxide from the air, and technical grade sodium hydroxide often contains some sodium carbonate, for example up to 0.5% by weight, preferably 0.1% to 0.4% by weight. By using such technical grade sodium hydroxide, a mixed hydroxide / carbonate is precipitated.
[0019] In one embodiment of the present invention, in step (a), the stoichiometric ratio of sodium hydroxide to the sum of nickel and other metals is about 2: 1. In this context, the term "about" refers to a ± 2 mol-% deviation of the hydroxide content from the ratio corresponding to the exact stoichiometric ratio. In the presence of aluminum, the amount of hydroxide may vary, also depending on the nature of the aluminum source.
[0020] In one embodiment of the present invention, the stoichiometric ratio of sodium carbonate to the sum of nickel and other metals is about 1: 1. In this context, the term "about" refers to a ±2 mol-% deviation of the carbonate content from the ratio corresponding to the exact stoichiometric ratio.
[0021] In step (a) a complexing agent is used, and the most economically advantageous complexing agent is ammonia, which can be used directly or in the form of an ammonium salt, such as ammonium sulfate. Ammonia is formed upon neutralization with the hydroxide.
[0022] The preferred molar ratio of ammonia to metal other than alkali metal is in the range of 1:10 to 1:1, more preferably 1:5 to 1:2.
[0023] Mixed metal hydroxides or mixed metal carbonates are precipitated by combining an aqueous solution containing nickel and a sulfate salt of at least one metal selected from cobalt and manganese with an aqueous solution of sodium hydroxide or sodium carbonate in the presence of ammonia or an ammonia salt. The mixed metal hydroxides or mixed metal carbonates are suspended (slurried) in a continuous phase containing sodium sulfate, and trace amounts of nickel and either additional transition metal salts or excess sodium hydroxide and ammonia.
[0024] In one embodiment of the present invention, step (a) is carried out at a temperature ranging from 15°C to 80°C, preferably from 40°C to 70°C.
[0025] Step (a) is preferably carried out with a mixing operation such as stirring.
[0026] In step (a) a slurry of a precipitated mixed metal hydroxide or carbonate of nickel and at least one metal selected from cobalt and manganese is obtained. The mixed metal hydroxide or carbonate may contain additional metals, such as magnesium or aluminium.
[0027] In one embodiment of the present invention, step (a) is carried out at a pH value in the range of 10 to 13, preferably 11.1 to 12.5. The pH value is determined at 23°C and refers to the continuous phase.
[0028] In one embodiment of the invention, the concentration of the mixed metal hydroxide or mixed metal carbonate may be increased by carrying out step (a) in a stirred vessel connected to a clarifier, such as a lamellar clarifier. By means of such a clarifier, the continuous phase may be removed from the stirred vessel. The continuous phase so removed may be combined with the filtrate from step (b).
[0029] In step (b), the precipitated nickel and at least one hydroxide or carbonate of a metal selected from cobalt and manganese are removed by filtration. The filtration can be carried out batchwise or continuously, for example, using a filter, in particular a filter press or a belt filter, by suction filtration or using a centrifuge. A filter press is preferred.
[0030] In the embodiment using a centrifuge, a supernatant and a precipitate are obtained. In the context of the present invention, in the subsequent steps, the supernatant takes the role of the filtrate and the precipitate takes the role of the filter cake without separate mention.
[0031] By filtering, a filter cake and a filtrate are obtained. The filter cake is preferably washed with water or with an aqueous sodium hydroxide or sodium carbonate solution according to step (a). After washing, the washing water can then be combined with the filtrate from step (b).
[0032] In one embodiment of (b), the filter cake from step (b) is pre-dried by blowing a gas such as nitrogen or air through the filter cake. The water so removed can be combined with the filtrate.
[0033] In one embodiment of step (b), the pH of the filtrate has a pH in the range of 10 to 13.5, preferably 11.1 to 12.5.
[0034] In step (c), ammonia is removed from the filtrate from step (b) by stripping in a distillation column or a fractionation column without or preferably with washing water, both expressions being used interchangeably in the context of the present invention.
[0035] While steps (a) and (b) may be performed continuously or batchwise, the distillation column or fractionation column in step (c) is preferably operated continuously and in a steady state.
[0036] In step (c), ammonia together with water is the lower boiling fraction and the aqueous solution containing sodium sulfate is the higher boiling fraction. Preferably, the concentration of ammonia (lower boiling fraction) in water is in the range of 0 to 10 ppm, preferably 1 to 5 ppm.
[0037] All data given in ppm refer to ppm by weight.
[0038] In one embodiment of the present invention, the distillation column or fractionation column in step (c) has a theoretical plate (theoretical tray) in the range of 10 to 50.
[0039] The distillation column or fractionation column in step (c) may have plates or trays with bubble caps.
[0040] In one embodiment of the present invention, the distillation column in step (c) is operated at a temperature ranging from 80°C to 120°C.
[0041] In one embodiment of the present invention, the distillation column in step (c) is operated at a pressure ranging from 10 mbar to 1.5 bar, ambient pressure is preferred.
[0042] The high boiling fraction usually contains a small amount of precipitate. Such precipitate may contain nickel hydroxide (or nickel carbonate, as the case may be) and, depending on the metal used in step (a), may contain at least one of cobalt or manganese.
[0043] The low-boiling (or "volatile") fraction from step (c) contains mainly ammonia and is then dissolved (washed out) with water and reused in step (a).
[0044] The high boiling fraction or liquid phase from step (c) is then subjected to step (d).
[0045] Step (d) comprises passing the high boiling fraction from step (c) (hereinafter also referred to as "remaining liquid phase") through a porous membrane, thereby obtaining a permeate. The membrane is preferably nanoporous.
[0046] The porous membrane may be made of a polymer, such as PES, PTFE, PVDF, PE, PP, each of which has an average pore size of 5 nm to 2 or even 3 μm. In another embodiment, the porous membrane may be made of a ceramic material such as Al 2 O 3 、TiO 2 、ZrO 2 , SiC or sintered metal. The more preferred ceramic membrane is made of Al 2 O 3 Made.
[0047] The polymer or ceramic membrane preferably has pores with an average diameter of 2 nanometers to 3 μm, preferably 20 to 400 nm and more preferably 50 to 100 nm.
[0048] To enhance the wear resistance of the ceramic membrane, a porous membrane comprising two or three membrane layers may be used, for example 800 nm, then 400 nm and finally 100 nm, or 400 nm, then 200 nm and finally 100 nm, and more preferably 400 nm, 200 nm and 50 nm.
[0049] In one embodiment of the present invention, step (d) is operated at a temperature ranging from 20°C to 95°C, preferably from 50°C to 70°C.
[0050] In one embodiment of the present invention, step (d) is operated at a pressure in the range of 2 to 6 bar (absolute pressure), preferably 2 to 5 bar (absolute pressure), and the high boiling fraction from step (c) is pressed through a porous membrane.
[0051] In another embodiment of the present invention, step (d) is operated at submerged pressure (eg up to 250 mbar) and the high boiling fraction from step (c) is pumped through the porous membrane.
[0052] From step (d) a permeate is obtained, hereinafter also referred to as brine. The brine preferably contains less than 10 ppm in total, preferably less than 0.1 ppm, more preferably less than the detection level of metals selected from nickel, cobalt and manganese. The brine is transparent and colorless to the naked eye. The concentration of sodium sulfate is preferably in the range of 5 to 20% by weight.
[0053] In one embodiment of the present invention, the process according to the invention comprises the additional step (d'): performing reverse osmosis. The reverse osmosis can be performed by passing the permeate from step (d) along a porous membrane, for example nanopores with a pore width of 2 nm or less, at a pressure of up to 120 bar. The temperature in the reverse osmosis step is preferably in the range of 20° C. to 35° C. By reverse osmosis, a permeate is obtained which is almost pure water. In addition, the retentate can contain up to 160 g / l, which corresponds to up to 15 wt.-%, of sodium sulphate. Reverse osmosis serves to remove water from the filtrate and to increase the concentration of sodium sulphate.
[0054] In step (e), the sodium sulfate of the permeate from step (d) or, if applicable, of the retentate from step (d′) is solidified by evaporation methods, for example in a spray tower or in an evaporative crystallizer.
[0055] Evaporative crystallizers are known per se. In one embodiment of the invention, the evaporative crystallization is carried out by one of the following methods:
[0056] - Falling film evaporation or
[0057] -Forced cycle crystallization.
[0058] In one embodiment of the present invention, the Na thus obtained is separated by centrifugation or filtration, preferably by centrifugation. 2 SO 4 Crystal removal. Drying can be carried out in a fluidized bed.
[0059] Preferably, the pH of the filtrate from step (d) or - if applicable - the retentate from step (d') is adjusted to a pH of 6.5 to 9.5, more preferably 6.8 to 8.0, with sulfuric acid before step (e). The closer the pH is to 10, the less corrosion problems are encountered in step (e). However, sodium sulfate containing a large amount of strong bases such as NaOH is not suitable when used as a builder.
[0060] In the spray tower, the salt water is sprayed to form droplets, from which the water evaporates. This forms a sodium sulfate powder that can be collected. By selecting the temperature and pressure, the droplet size and therefore the particle size of the resulting sodium sulfate can be controlled.
[0061] Each spray tower sprays through one or more nozzles. Suitable nozzles are, for example, high-pressure drum atomizers, rotary atomizers, three-fluid nozzles, single-fluid nozzles and two-fluid nozzles, single-fluid nozzles and two-fluid nozzles being preferred. The first fluid is the brine from step (d), and the second fluid is a compressed hot gas (also referred to as a hot gas inlet stream), for example with a pressure of 1.1 to 7 bar. The hot gas inlet stream may have a temperature in the range of at least 125°C to 250°C, preferably 150°C to 250°C, even more preferably 160°C to 220°C.
[0062] In one embodiment of the present invention, a single effect spray dryer is used. In an alternative embodiment, a multiple effect spray dryer may be used.
[0063] In one embodiment of step (e), the brine obtained from step (d) is introduced in the form of droplets.In one embodiment of the invention, the droplets formed during spray drying have an average diameter in the range of 10 to 200 μm, preferably 15 to 150 μm.
[0064] In one embodiment of the invention, the offgas leaving the spray tower may have a temperature in the range of 40° C. to 140° C., preferably 80° C. to 110° C., but in any case cooler than the hot gas stream. Preferably, the temperature of the offgas leaving the drying vessel is the same as the temperature of the solid product present in the drying vessel.
[0065] In one embodiment of the present invention, the pressure in the spray tower in step (e) is atmospheric pressure ±100 mbar, preferably atmospheric pressure ±20 mbar, for example 1 mbar lower than atmospheric pressure.
[0066] In a preferred evaporative crystallizer, the body of the crystallization vessel simultaneously carries out evaporation and crystallization. The process is driven by a heat exchanger in a pump loop, wherein steam is used to heat the circulating solution. Fresh brine feed enters this loop before passing through the heat exchanger. The heated suspension reenters the crystallization body and releases its heat by evaporation. The resulting concentration increase causes crystallization to occur. The steam leaving the crystallizer body is preferably recompressed by an MVR ("mechanical vapor recompression") fan and can therefore be used to further drive the operation of the crystallizer. With this particular embodiment, there is no need to consume fresh and expensive steam.
[0067] By carrying out the process of the present invention, sodium sulfate is obtained which is very suitable as a builder for the manufacture of laundry detergents, having a whiteness greater than 85% measured by standard reflectance measurement (e.g., Kett C-100). Thus, the sodium sulfate obtained has very good whiteness and no malodor is detectable. The chloride content is preferably 500 ppm or less, more preferably 50 ppm or less.
[0068] Further disclosed is a device in which the method of the present invention can be carried out. Such a device of the present invention comprises a plurality of components:
[0069] (A) at least one stirred tank reactor connected to
[0070] (B) Filtration equipment,
[0071] (C) a distillation column,
[0072] (D) a container including a ceramic membrane, and
[0073] (E) A vessel for removing water by evaporation, for example an evaporative crystallizer (E1) as a tubular heat exchanger or a spray dryer ("spray tower") (E2).
[0074] The above components are connected in such a way that a fluid can subsequently flow through them. This means that a fluid can flow through these components in the order of (A), (B), (C), (D) and (E). The fluid can be water containing sodium sulphate. However, in component (E), solid sodium sulphate and water or concentrated brine are obtained.
[0075] The vessel (E) may be selected from an evaporative crystallizer and a spray tower.
[0076] The porous membrane in component (D) may be selected from polymer membranes and ceramic membranes.
[0077] Component (D) may comprise a unit comprising two or more membranes traversed by the permeate.
[0078] The device may additionally comprise a component (D') having a membrane for reverse osmosis.
[0079] Examples
[0080] The following apparatus is used: a 10-1 stirred tank reactor (A.1) with baffles, overflow system, laminar clarifier and stirrer, connected to a filter press (B.1). The filtrate can be transferred to a fractionation column (C.1). The low-boiling fraction is transferred to a first vessel with a porous ceramic filter (D.1), a reverse osmosis unit (D'.1), and the retentate is transferred from there to a crystallizer (E.1) or a spray dryer (E.2).
[0081] Step (a.1):
[0082] Synthesis of Precursor TM-OH.1
[0083] A stirred tank reactor (A.1) was filled with deionized water and 49 g of ammonium sulfate per kg of water. The solution was temperature adjusted to 55° C. and the pH value was adjusted to 12 by adding aqueous sodium hydroxide solution.
[0084] The coprecipitation reaction was started by simultaneously feeding an aqueous transition metal sulfate solution and an aqueous sodium hydroxide solution at a flow rate ratio of 1.8, and the total flow rate resulted in a residence time of 8 hours. The transition metal solution contained Ni, Co and Mn in a molar ratio of 8.5:1.0:0.5 and a total transition metal concentration of 1.65 mol / kg. The aqueous sodium hydroxide solution was a 25 wt.% sodium hydroxide solution and a 25 wt.% ammonia solution in a weight ratio of 6. The pH value was maintained at 12 by feeding the aqueous sodium hydroxide solution alone. From the start of all feeds, the mother liquor was continuously removed. After 33 hours, all feed streams were stopped.
[0085] Step (b.1): A mixed transition metal (TM) oxyhydroxide precursor is obtained by filtering the resulting suspension on a filter press (B.1), washing with 1% by weight NaOH solution, drying at 120° C. in air and sieving.
[0086] The filtrate from step (b.1) was combined with the mother liquor and washing water withdrawn in step (a.1). The combined filtrate thus obtained had a pH value of 12.0.
[0087] Step (c.1):
[0088] The combined filtrate from step (b.1) was transferred to a fractionation column (C.1). A distillation column with trays with bubble caps and 15 theoretical plates was used as fractionation column (C.1). Step (c.1) was operated continuously. The low-boiling fraction was a 15% by weight aqueous ammonia solution, and the "high-boiling fraction" was a slightly turbid Na+ solution with a pH of 12. 2 SO 4 Aqueous solution.
[0089] Step (d.1)
[0090] The slightly turbid solution from step (c.1) was cooled to 50°C and transferred to a porous ceramic Al 2 O 3 20-1 container (D.1) of the membrane unit: three membranes with an average pore size of 800 nm, then 400 nm and finally 100 nm. A pressure of 3 bar was applied. A transparent and colorless permeate was obtained.
[0091] After step (d.1), sulfuric acid was added to the permeate from step (d.1) to adjust the pH to 7.0.
[0092] Step (d'.1):
[0093] The neutralized permeate from step (d.1) is cooled to 25°C and subjected to reverse osmosis. Water is removed from the permeate of step (d'.1) at a pressure of 100 bar, thereby obtaining the permeate of step (d'.1) and a retentate. The retentate is then transferred to step (e.1).
[0094] Step (e.1)
[0095] The neutralized, clear and colorless filtrate from step (d.1) is then transferred to a tubular heat exchanger (E.1) used as a falling film evaporator. The solution is heated to 100° C. to 110° C. by passing it repeatedly through the tubular heat exchanger and the water evaporates. The solution, thus concentrated but still free of crystals, enters the crystallizer unit. Here, the solution is pumped to another heat exchanger, in which it is superheated to 110° C. to 120° C. Upon re-entering the crystallizer, the water evaporates and the Na 2 SO 4 Crystals precipitate. The suspension is drawn off from the crystallizer with the aid of a pump and the crystals are separated from the suspension by a laboratory-scale belt filter. The whiteness of these crystals is excellent and they have no bad odor.
[0096] Step (e.2)
[0097] The neutralized transparent and colorless filtrate from step (d.1) is then transferred to a single-effect laboratory spray dryer through a spray nozzle. Air is used as the gas for the nozzle. A mist is formed. The spray tower is operated in a co-current mode of gas flow and mist. The gas temperature is 200°C. The filtrate is introduced through a nozzle having a pressure of 2500 kPa. White odorless Na 2 SO 4 Powder, average particle size 10μm.
[0098] Na 2 SO 4 The nickel content was below detection levels in every case.
Claims
1. A method for producing crystalline sodium sulfate, the method comprising: The following steps are involved: (a) combining an aqueous solution containing nickel and a sulfate salt of at least one metal selected from cobalt and manganese with an aqueous solution of sodium hydroxide or sodium carbonate in a stoichiometric ratio of about 1:2 or 1:1, respectively, in the presence of ammonia or an ammonia salt, (b) removing the precipitated nickel and the hydroxide or carbonate of the at least one metal selected from cobalt and manganese by filtration, (c) removing the ammonia from the filtrate from step (b) by stripping in a distillation column, (d) passing the remaining liquid phase through the porous membrane, thereby obtaining a permeate, and (e) removing water from the permeate from step (d) by evaporation.
2. The method according to claim 1, in, The filtrate in step (c) has a pH value in the range of 10 to 13.
3. The method according to claim 1 or 2, in, The evaporation method in step (e) is selected from spray drying and evaporative crystallization.
4. The method according to any one of the preceding claims, in, The chloride content of the sulfate filtrate after step (d) is in the range of 0 to 10 ppm by weight relative to the filtrate.
5. The method according to any one of the preceding claims, in, In step (a), by introducing MgSO 4 、Al 2 (SO 4 ) 3 、NaAl(OH) 4 、NaAl(SO 4 ) 2 and KAl(SO 4 ) 2 At least one of aluminum and magnesium is additionally included in the precipitate.
6. The method according to any one of the preceding claims, in, In step (d) a pressure of up to 5 atmospheres is used.
7. The method according to any one of the preceding claims, in, Between steps (d) and (e) a reverse osmosis (d') is carried out.
8. The method according to any one of the preceding claims, in, Prior to step (e), the permeate from step (d) or, if applicable, the retentate from step (d′) is adjusted to a pH value of 6.5 to 9.5 with sulphuric acid.
Citation Information
Patent Citations
Ternary precursor production wastewater mother liquor treatment system and method
CN112299638A
Process for the reclamation of process water from process wastewater generated in the battery manufacturing industry and other metals related industries
US6001246A
Method for preparing cathode active material precursor for secondary battery, and preparation apparatus using same