Hollow particles
By adjusting the shell polymer monomer composition of the hollow particles and increasing their true density and C value, the problems of existing hollow particles being easily swelled and porosity decreased under solvents are solved, and the solvent resistance and molding effect are improved.
Patent Information
- Application Number
- CN202380027664.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-05
AI Technical Summary
The existing hollow particles are prone to swelling in the presence of solvents, and their porosity is reduced, resulting in insufficient addition effect in molded materials, especially poor solvent resistance.
By designing the monomer composition of shell polymer, the true density reaches 1.16g/cm3 or above, and by a specific C value (calculated from the proportion of the true density and the monofunctional monomer content in shell polymer), it reaches 0.94 or above, and the cross-section is optimized. The ratio of linked monomers and functional monomers increases the solvent resistance of hollow particles.
The excellent solvent resistance of hollow particles is achieved, ensuring sufficient lightweight and low dielectric loss tangent effect in the molded material.
Smart Images

Figure BDA0005042672470000281
Abstract
Description
Technical Field
[0001] The invention relates to hollow particles. Background Art
[0002] Hollow particles such as hollow resin particles produced by polymerizing polymerizable monomers are particles having a cavity inside the particles. Compared with solid particles whose interior is substantially filled with resin, etc., hollow particles can scatter light well and reduce the transmittance of light. Therefore, they are widely used in water-based coatings, paper coating compositions, and the like as organic pigments and masking agents with excellent optical properties such as opacity and whiteness. They are also used as additives for molded bodies such as reflectors, heat insulating materials, and sound insulating materials (additives added to the molding resin), etc.
[0003] As a technology involving such hollow particles, for example, Patent Document 1 discloses a hollow resin particle having a shell portion and a hollow portion surrounded by the shell portion, wherein the shell portion includes an aromatic polymer (P1) obtained by polymerizing a monomer composition containing an aromatic crosslinking monomer (a), an aromatic monofunctional monomer (b), and a (meth)acrylate monomer (c) represented by a specific formula (1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: International Publication No. 2021 / 085189. Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, according to the research conducted by the present inventors, it is known that the hollow particles disclosed in Patent Document 1 have poor solvent resistance. When the hollow particles are used together with a solvent, the hollow particles are easily swelled by the solvent, and the porosity of the hollow particles is easily reduced. As a result, for example, when the hollow particles are mixed with a molding resin, the effect of adding the hollow particles (such as weight reduction and low dielectric loss tangent) becomes insufficient.
[0009] An object of the present invention is to provide hollow particles having excellent solvent resistance.
[0010] Solutions for solving problems
[0011] The present inventors have conducted studies to achieve the above object and have found that, for hollow particles having a shell composed of a shell polymer containing crosslinkable monomer units and a hollow portion, by setting the true density to 1.16 g / cm 3 As described above, the C value calculated by the specific formula (1) is 0.94 or more, and the above-mentioned object can be achieved, thereby completing the present invention.
[0012] That is, according to the present invention, there is provided a hollow particle having a shell containing a resin and a hollow part surrounded by the shell,
[0013] The above resin is composed of a shell polymer containing crosslinkable monomer units,
[0014] The true density of the above hollow particles is 1.16 g / cm 3 above,
[0015] The value of C of the hollow particles calculated by the following formula (1) is 0.94 or more,
[0016] C=A×(100-B) / 100 Formula (1)
[0017] (In the above formula (1), A represents the value of the true density of the hollow particles (unit: g / cm 3 ), B represents the content ratio of the monofunctional monomer unit in the shell polymer (unit: mass %)).
[0018] In the hollow particles of the present invention, it is preferred that the shell polymer contains a heteroatom-containing monomer unit, and the content ratio of the heteroatom-containing monomer unit in the shell polymer is 80% by mass or more.
[0019] In the hollow particles of the present invention, it is preferred that the ratio of hollow particles precipitated when immersed in toluene for 48 hours is less than 5% by mass.
[0020] In the hollow particles of the present invention, it is preferred that the ratio of hollow particles precipitated when immersed in methyl ethyl ketone for 24 hours is less than 5% by mass.
[0021] In the hollow particles of the present invention, it is preferred that the ratio of hollow particles precipitated when immersed in acetone for 24 hours is less than 5% by mass.
[0022] The hollow particles of the present invention preferably have a porosity of 60% or more.
[0023] In the hollow particles of the present invention, the shell polymer preferably contains trifunctional or higher crosslinkable monomer units and bifunctional crosslinkable monomer units as the crosslinkable monomer units.
[0024] In the hollow particles of the present invention, the ratio of the content of the bifunctional crosslinking monomer unit to the content of the trifunctional or higher heteroatom-containing crosslinking monomer unit in the shell polymer is preferably 10:90 to 98:2 in terms of the mass ratio of "bifunctional crosslinking monomer unit: trifunctional or higher heteroatom-containing crosslinking monomer unit".
[0025] The hollow particles of the present invention preferably have a volume average particle diameter (Dv) of 1 to 12 μm.
[0026] Effects of the Invention
[0027] The present invention can provide hollow particles having excellent solvent resistance. DETAILED DESCRIPTION
[0028] <Hollow particles>
[0029] The hollow particles of the present invention have a shell containing a resin and a hollow part surrounded by the shell, wherein the resin is composed of a shell polymer containing a crosslinkable monomer unit, and the true density of the hollow particles is 1.16 g / cm 3 As described above, the value of C of the hollow particles calculated by the following formula (1) is 0.94 or more.
[0030] C = A × (100-B) / 100 Formula (1) (In the above formula (1), A represents the value of the true density of the hollow particles (unit: g / cm 3 ), B represents the content ratio of the monofunctional monomer unit in the shell polymer (unit: mass %)).
[0031] The shell of the hollow particles of the present invention contains a resin composed of a shell polymer.
[0032] The shell polymer is a polymer for forming the shell of the hollow particles, and contains a crosslinkable monomer unit. The crosslinkable monomer forming the crosslinkable monomer unit is a monomer having two or more polymerizable functional groups and forming a crosslink bond in the resin through a polymerization reaction. As the crosslinkable monomer, a compound having at least one ethylenically unsaturated bond as a polymerizable functional group is generally used.
[0033] Examples of the crosslinkable monomer that forms the crosslinkable monomer unit include a crosslinkable hydrocarbon monomer and a heteroatom-containing crosslinkable monomer.
[0034] The crosslinkable hydrocarbon monomer is not particularly limited, and examples thereof include bifunctional crosslinkable hydrocarbon monomers such as divinylbenzene, divinylbiphenyl, and divinylnaphthalene. Among them, divinylbenzene is preferred.
[0035] The heteroatom-containing crosslinking monomer is not particularly limited, and examples thereof include: difunctional heteroatom-containing crosslinking monomers such as diallyl phthalate, allyl (meth)acrylate [referring to allyl acrylate and / or allyl methacrylate, the same below], ethylene glycol di(meth)acrylate, and pentaerythritol di(meth)acrylate; trifunctional or higher heteroatom-containing crosslinking monomers such as trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and dipentaerythritol poly(meth)acrylate. Among these, ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate and pentaerythritol tri(meth)acrylate are preferred, ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate and pentaerythritol tetra(meth)acrylate are more preferred, ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate and pentaerythritol tetramethacrylate are further preferred, and ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate are particularly preferred.
[0036] As the crosslinking monomer, a crosslinking hydrocarbon monomer, ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate and pentaerythritol tri(meth)acrylate are preferred; divinylbenzene, ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate and pentaerythritol tetra(meth)acrylate are more preferred; divinylbenzene, ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate and pentaerythritol tetramethacrylate are further preferred; ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate are particularly preferred.
[0037] The crosslinking monomers can be used alone or in combination of two or more. In the hollow particles of the present invention, the shell polymer preferably contains a difunctional crosslinking monomer unit and a trifunctional or higher crosslinking monomer, more preferably contains a difunctional crosslinking monomer unit and a trifunctional or higher heteroatom-containing crosslinking monomer unit, and further preferably contains a difunctional heteroatom-containing crosslinking monomer unit and a trifunctional or higher heteroatom-containing crosslinking monomer unit. In addition, there is no particular limitation on the trifunctional or higher crosslinking monomer, preferably a trifunctional to hexafunctional crosslinking monomer, more preferably a trifunctional to pentafunctional crosslinking monomer, further preferably a trifunctional to tetrafunctional crosslinking monomer, and particularly preferably a trifunctional crosslinking monomer. In addition, in the hollow particles of the present invention, the shell polymer can also contain a crosslinking hydrocarbon monomer unit and a heteroatom-containing crosslinking monomer unit.
[0038] The content of the bifunctional crosslinkable monomer unit in the shell polymer is not particularly limited, but is preferably 10 to 98% by mass, more preferably 25 to 95% by mass, further preferably 40 to 90% by mass, particularly preferably 50 to 85% by mass, and most preferably 55 to 80% by mass.
[0039] The content of the trifunctional or higher heteroatom-containing crosslinkable monomer units in the shell polymer is not particularly limited, but is preferably 90 to 2% by mass, more preferably 75 to 5% by mass, further preferably 60 to 10% by mass, particularly preferably 50 to 15% by mass, and most preferably 45 to 20% by mass.
[0040] The ratio of the content ratio of the bifunctional crosslinking monomer unit to the content ratio of the trifunctional or higher heteroatom-containing crosslinking monomer unit in the shell polymer is not particularly limited, but the mass ratio of "bifunctional crosslinking monomer unit: trifunctional or higher heteroatom-containing crosslinking monomer unit" is preferably 10:90 to 98:2, more preferably 25:75 to 95:5, further preferably 40:60 to 90:10, particularly preferably 50:50 to 85:15, and most preferably 55:45 to 80:20.
[0041] The shell polymer may be substantially composed of only crosslinkable monomer units, or may contain monofunctional monomer units in addition to the crosslinkable monomer units.
[0042] The monofunctional monomer forming the monofunctional monomer unit is a monomer having only one polymerizable functional group, and generally a compound having an ethylenically unsaturated bond as the polymerizable functional group is used. Examples of the monofunctional monomer forming the monofunctional monomer unit include monofunctional hydrocarbon monomers and heteroatom-containing monofunctional monomers.
[0043] The monofunctional hydrocarbon monomer is not particularly limited, and examples thereof include aromatic vinyl monomers such as styrene, ethylvinylbenzene, vinyltoluene, α-methylstyrene, p-methylstyrene, and halogenated styrene; monoolefin monomers such as ethylene, propylene, butene, and 4-methyl-1-pentene; and diene monomers such as butadiene and isoprene. Among these, styrene and ethylvinylbenzene are preferred.
[0044] The heteroatom-containing monofunctional monomer is not particularly limited, and examples thereof include: hydrophilic monofunctional monomers; acrylic monovinyl monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; carboxylic acid vinyl ester monomers such as vinyl acetate; vinyl halide monomers such as vinyl chloride; vinylidene halide monomers such as vinylidene chloride; vinyl pyridine monomers, etc.
[0045] The hydrophilic monofunctional monomer preferably has a solubility of 1% by mass or more in water. The hydrophilic monofunctional monomer is not particularly limited, and examples thereof include monofunctional monomers having a hydrophilic group such as an acid group-containing monomer, a hydroxyl group-containing monomer, an amide group-containing monomer, and a polyoxyethylene group-containing monomer.
[0046] An acid group-containing monomer refers to a monomer containing an acid group. The acid group mentioned here also includes any one of a proton donor group (Brönsted acid group) and an electron pair acceptor group (Lewis acid group). As an acid group-containing monomer, there is no particular limitation as long as it has an acid group, and examples thereof include carboxyl group-containing monomers and sulfonic acid group-containing monomers. Examples of carboxyl group-containing monomers include: ethylenically unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, butenetricarboxylic acid, etc.; monoalkyl esters of unsaturated dicarboxylic acids such as monoethyl itaconate, monobutyl fumarate, and monobutyl maleate, etc. Examples of sulfonic acid group-containing monomers include styrene sulfonic acid, etc.
[0047] As a hydroxyl group-containing monomer, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. are mentioned, for example.
[0048] Examples of the amide group-containing monomer include acrylamide and dimethylacrylamide.
[0049] Examples of the polyoxyethylene group-containing monomer include methoxypolyethylene glycol (meth)acrylate and the like.
[0050] The monofunctional monomer units can be used alone or in combination of two or more.
[0051] The content of the crosslinkable monomer unit in the shell polymer is not particularly limited, preferably 82% by mass or more, more preferably 85% by mass or more, further preferably 88% by mass or more, particularly preferably 90% by mass or more, and most preferably 95% by mass or more. By making the content of the crosslinkable monomer within the above range, the covalent bond network is densely distributed in the shell, and the generation of the interconnecting pores and shell defects of the shell is also suppressed, resulting in the mechanical strength of the hollow particles becoming excellent. In addition, by making the content of the crosslinkable monomer within the above range, more excellent solvent resistance can be obtained.
[0052] The content ratio of the monofunctional monomer unit in the shell polymer is not particularly limited, but is preferably 0 to 18% by mass, more preferably 0 to 15% by mass, further preferably 0 to 12% by mass, particularly preferably 0 to 10% by mass, and most preferably 0 to 5% by mass, from the viewpoint of obtaining the mechanical strength of the hollow particles and better solvent resistance.
[0053] In addition, the value of the content ratio of the crosslinking monomer unit in the shell polymer (unit: mass %) is represented by (100-B) in the formula (1) described below, and the value of the content ratio of the monofunctional monomer unit in the shell polymer (unit: mass %) is represented by B in the formula (1) described below.
[0054] The shell polymer may contain a heteroatom-containing monomer unit. Examples of the heteroatom-containing monomer that forms the heteroatom-containing monomer unit include the above-mentioned heteroatom-containing crosslinking monomer and heteroatom-containing monofunctional monomer.
[0055] The content of the heteroatom-containing monomer unit in the shell polymer is not particularly limited, but is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 70% by mass or more, and particularly preferably 80% by mass or more from the viewpoint of obtaining better solvent resistance. By making the content of the heteroatom-containing monomer unit within the above range, the solvent resistance of the hollow particles to not only polar solvents but also non-polar solvents is further improved.
[0056] When extremely high resistance to non-polar solvents is required, the content of the heteroatom-containing monomer units is preferably 82.5% by mass or more, more preferably 85% by mass or more, further preferably 87.5% by mass or more, further preferably 90% by mass or more, particularly preferably 92.5% by mass or more, and most preferably 95% by mass or more.
[0057] On the other hand, when excellent electrical insulation is required, the content of the heteroatom-containing monomer unit is preferably 96 mass % or less, more preferably 93 mass % or less, further preferably 90 mass % or less, particularly preferably 87 mass % or less, and most preferably 84 mass % or less.
[0058] The hollow particles of the present invention are particles having a shell (shell) containing the above-mentioned resin and a hollow portion surrounded by the shell. In the present invention, the hollow portion is a hollow space clearly distinguished from the shell of the hollow particles formed by the resin. The hollow particles of the present invention may have one or more hollow portions, and in order to maintain a good balance between high porosity and mechanical strength, preferably only one hollow portion. In the hollow particles of the present invention, the proportion of particles having only one hollow portion is preferably 90% by mass or more, more preferably 95% by mass or more.
[0059] The hollow particles of the present invention are generally hollow particles in which the shell has no communicating holes and shell defects, and the hollow part is isolated from the outside of the particle by the shell, but may also be hollow particles in which the shell has one or more communicating holes, and the hollow part is connected to the outside of the particle via the communicating holes. In addition, the shell of the hollow particle and the partition wall separating adjacent hollow parts in the case of having two or more hollow parts may be porous, in which case the hollow part has a size that can be clearly distinguished from a plurality of microscopic spaces uniformly dispersed in the porous structure.
[0060] The hollow part of the hollow particles of the present invention may be filled with a gas such as air, or may contain a solvent.
[0061] The shape of the hollow particles of the present invention is not particularly limited as long as a hollow portion is formed inside. The outer shape of the hollow particles is not particularly limited, but a spherical shape is preferred from the viewpoint of ease of production.
[0062] The outer shape of the hollow particles can be confirmed by, for example, observing the particles with SEM or TEM. In addition, the internal shape of the hollow particles can be confirmed by, for example, observing the cross section of the particles with SEM or observing the particles with TEM.
[0063] The average roundness of the hollow particles of the present invention can be 0.950 to 0.995. In addition, the hollow particles of the present invention also have excellent pressure resistance due to the small proportion of particles with a roundness of 0.85 or less. Particles with a roundness of 0.85 or less are typically particles that have undergone deformations such as depressions and cracks, and are sometimes referred to as "irregular-shaped particles" in the present invention. Such irregular-shaped particles are easily subjected to external pressure locally, and therefore have poor pressure resistance compared to spherical particles. Furthermore, irregular-shaped particles have the problem of being easily agglomerated and having poor dispersibility when dispersed in a binder resin compared to spherical particles. When irregular-shaped particles are dispersed in a binder resin, it is easy to generate agglomerates and external pressure is easily applied to the agglomerates, so the pressure resistance is worse. Therefore, by reducing the proportion of irregular-shaped particles contained in the hollow particles, the dispersibility and pressure resistance of the hollow particles can be improved.
[0064] The hollow particles of the present invention may contain a small amount of particles with low roundness due to particle breakage, deformation, etc. as impurities. Among 100 mass% of the hollow particles of the present invention, the proportion of particles with a roundness of 0.85 or less is preferably 10 mass% or less, more preferably 7 mass% or less, further preferably 5 mass% or less, further preferably 4 mass% or less, and particularly preferably 3 mass% or less.
[0065] The roundness is defined as the value obtained by dividing the diameter of a circle having the same area as the projection image of the particle (equivalent circular area diameter) by the diameter of a circle having the same circumference as the projection image of the particle (equivalent circular circumference diameter). In the case where the particle is a perfect sphere, the roundness is 1, and the more complex the surface shape of the particle, the smaller the roundness value.
[0066] In the present invention, the roundness is measured using a flow particle imaging measuring device with an image resolution of 0.185 μm / pixel. As a flow particle imaging measuring device, for example, the trade name "IF-3200" manufactured by JASCO INTERNATIONAL Co., Ltd. can be preferably used. The measurement sample is prepared by, for example, dispersing a mixed solution obtained by adding 0.10 to 0.12 g of hollow particles to an aqueous solution of sodium linear alkylbenzene sulfonate (concentration 0.3%) for 5 minutes using an ultrasonic cleaner. The average roundness is the average value of the roundness of 1000 to 3000 particles selected at random.
[0067] The true density of the hollow particles of the present invention is 1.16 g / cm 3 The present invention was completed by finding that the hollow particles have excellent solvent resistance when the true density and C values are within the above ranges.
[0068] In this specification, the true density of hollow particles refers to the density of only the shell part of the hollow particles. The true density of hollow particles is specifically measured by the following method. The hollow particles are crushed in advance and then placed in a container with a capacity of 100 cm 3 A volumetric flask is filled with about 10 g of hollow particle fragments, and the mass of the filled fragments is accurately weighed. Next, isopropyl alcohol is added to the volumetric flask in the same manner as the above-mentioned apparent density measurement, and the mass of isopropyl alcohol is accurately weighed. The true density (g / cm2) of the hollow particles is calculated based on the following formula (I): 3 ).
[0069] Hollow particle true density (g / cm 3 ) = [mass of the hollow particle fragments] ÷ (100 - [mass of isopropyl alcohol] ÷ [density of isopropyl alcohol at the measurement temperature]) (I)
[0070] The true density of the hollow particles of the present invention is only 1.16 g / cm 3 The above values are not particularly limited, but from the viewpoint of obtaining excellent mechanical strength and more excellent solvent resistance of the hollow particles, the molecular weight is preferably 1.16 to 1.25 g / cm 3 , more preferably 1.16 to 1.22 g / cm 3 , more preferably 1.16 to 1.20 g / cm 3In addition, when extremely excellent solvent resistance is required, the true density of the hollow particles is preferably 1.17 g / cm 3 More preferably 1.18 g / cm 3 More preferably, 1.19 g / cm 3 Above, particularly preferably 1.195 g / cm 3 above.
[0071] The value of C of the hollow particles of the present invention calculated from the following formula (1) is 0.94 or more.
[0072] C=A×(100-B) / 100 Formula (1)
[0073] In the above formula (1), A represents the value of the true density of the hollow particles (unit: g / cm 3 ), B represents the content ratio of the monofunctional monomer unit in the shell polymer (unit: mass %).
[0074] The value of C calculated by formula (1) of the hollow particles of the present invention is not particularly limited as long as it is 0.94 or more. From the viewpoint of obtaining excellent electrical insulation and better solvent resistance, it is preferably 0.96 to 1.25, more preferably 0.98 to 1.24, further preferably 1.00 to 1.22, particularly preferably 1.03 to 1.21, and most preferably 1.06 to 1.20.
[0075] The true density of the hollow particles and the value of C calculated from the formula (1) can be adjusted by adjusting the monomer composition of the shell polymer.
[0076] The porosity of the hollow particles of the present invention can be, for example, 60% or more. According to the present invention, the porosity of the hollow particles can be preferably 40 to 95%, more preferably 50 to 90%, further preferably 55 to 85%, and particularly preferably 60 to 80%. By making the porosity within the above range, when, for example, the hollow particles of the present invention are mixed with a molding resin and pressure-molded, the addition effect of the hollow particles (for example, light weight, low dielectric loss tangent) can be fully achieved.
[0077] The porosity of hollow particles is calculated based on the apparent density D of the hollow particles. 1 and true density D 0 In addition, the apparent density D 1 It is equivalent to the density of the entire hollow particle when the hollow part is regarded as a part of the hollow particle. In addition, when the hollow part of the hollow particle contains components other than the components constituting the shell (shell polymer, etc.), it is considered that most of the components other than the components constituting the shell come from the residual solvent, so it is considered that the density of the components other than the components constituting the shell is equal to the true density D of the hollow particle.0 Specifically, the apparent density D is calculated using the mass of the hollow particles including the mass of the components other than the components constituting the shell as the mass of the hollow particles. 1 Next, using the apparent density D calculated in this way 1 To calculate the porosity of hollow particles.
[0078] The apparent density of hollow particles is D 1 The determination method is as follows. First, in a volume of 100 cm 3 Fill the volumetric flask to about 30 cm 3 The mass of the hollow particles was accurately weighed. Next, the volumetric flask filled with the hollow particles was accurately filled to the mark with isopropyl alcohol while being careful not to mix in bubbles. The mass of the isopropyl alcohol added to the volumetric flask was accurately weighed, and the apparent density D of the hollow particles was calculated based on the following formula (II): 1 (g / cm 3 ).
[0079] The apparent density of hollow particles is D 1 (g / cm 3 ) = [mass of hollow particles] ÷ (100 - [mass of isopropyl alcohol] ÷ [density of isopropyl alcohol at the measurement temperature]) (II)
[0080] The porosity (%) of the hollow particles is calculated based on the apparent density D of the hollow particles. 1 and true density D 0 It is calculated by the following formula (III).
[0081] Porosity of hollow particles (%) = 100 - [apparent density of hollow particles D 1 ]÷[True density of hollow particles D 0 ]×100 (III)
[0082] The volume average particle size (Dv) of the hollow particles of the present invention is not particularly limited, but is preferably 1 to 12 μm, more preferably 1.5 to 11 μm, further preferably 2 to 10 μm, particularly preferably 2.2 to 9.5 μm, and most preferably 2.5 to 9 μm. In addition, when added to a substrate with a thin film thickness, the volume average particle size (Dv) is preferably 8 μm or less, more preferably 7 μm or less, further preferably 6 μm or less, particularly preferably 5 μm or less, and most preferably 4 μm or less.
[0083] The particle size distribution (Dv / Dn) (volume average particle size (Dv) / number average particle size (Dn)) of the hollow particles of the present invention is not particularly limited, and is preferably 1.02 to 2.00, more preferably 1.04 to 1.60, further preferably 1.06 to 1.50, particularly preferably 1.08 to 1.40, and most preferably 1.10 to 1.30. By making the particle size distribution (Dv / Dn) of the hollow particles within the above range, when, for example, the hollow particles of the present invention are mixed with a molding resin and press-molded, the deformation of the hollow particles can be suppressed, and the addition effect of the hollow particles (for example, light weight, low dielectric loss tangent) can be fully achieved.
[0084] For the volume average particle size (Dv) and number average particle size (Dn) of the hollow particles, the particle size of the hollow particles can be measured by, for example, a laser diffraction particle size distribution measuring device, and the number average value and volume average value thereof are calculated, respectively, and the obtained values are used as the number average particle size (Dn) and volume average particle size (Dv) of the particles. The particle size distribution (Dv / Dn) is the value obtained by dividing the volume average particle size (Dv) by the number average particle size (Dn).
[0085] The volume average particle size (Dv) and particle size distribution (Dv / Dn) of the hollow particles can be adjusted by, for example, adjusting the monomer composition of the shell polymer, the type and amount of the dispersion stabilizer used when producing the hollow particles by suspension polymerization, and the suspension conditions.
[0086] The hollow particles of the present invention are composed of a shell polymer containing a crosslinkable monomer unit, and the true density is 1.16 g / cm 3 The value of C calculated from the above formula (1) is 0.94 or more, which indicates excellent solvent resistance. Specifically, the hollow particles of the present invention have excellent solvent resistance such as resistance to swelling in nonpolar solvents such as toluene and polar solvents such as methyl ethyl ketone and acetone.
[0087] The hollow particles of the present invention preferably have a precipitated ratio of less than 5% by mass when immersed in toluene for 48 hours, and more preferably have a precipitated ratio of less than 5% by mass when immersed in toluene for 240 hours.
[0088] Furthermore, the hollow particles of the present invention preferably have a ratio of less than 5% by mass of hollow particles precipitated when immersed in methyl ethyl ketone for 24 hours.
[0089] Furthermore, the hollow particles of the present invention preferably have a ratio of less than 5% by mass of hollow particles precipitated when immersed in acetone for 24 hours.
[0090] The thermal decomposition starting temperature of the hollow particles of the present invention is preferably 150 to 400° C., more preferably 200 to 350° C. The hollow particles having a thermal decomposition starting temperature within the above range have excellent heat resistance. The thermal decomposition starting temperature of the hollow particles is the temperature at which the weight is reduced by 5%. The thermal decomposition starting temperature of the hollow particles can be measured by a TG-DTA device under the conditions of an air flow rate of 230 mL / min and a heating rate of 10° C. / min in an air environment.
[0091] As the purpose of the hollow particles of the present invention, for example, low dielectric materials, heat insulating materials, sound insulating materials and reflective materials used in various fields such as automobiles, electrical, electronic, construction, aviation, aerospace, etc., food containers, shoes such as sports shoes and sandals, home appliance parts, bicycle parts, stationery, tools, etc. can be cited. Among them, the hollow particles of the present invention are suitable for use as additives for achieving low transmission loss in the field of electrical or electronic. For example, the hollow particles of the present invention are suitable for use as circuit substrate materials. Specifically, by making the insulating resin layer of the circuit substrate contain the hollow particles of the present invention, the transmission loss of the circuit substrate can be reduced.
[0092] In addition, the hollow particles of the present invention are also suitable for use as additives in semiconductor materials such as interlayer insulating materials, dry film resists, solder resists, bonding wires, bonding sheets, magnetic wires, semiconductor sealing materials, epoxy sealing materials, mold under fillers, bottom fillers, chip bonding pastes, buffer coating materials, copper-clad laminates, flexible substrates, high-frequency device modules, antenna modules, and vehicle-mounted radars. Among these, it is also particularly preferred as additives in semiconductor materials such as interlayer insulating materials, solder resists, bonding sheets, magnetic wires, epoxy sealing materials, bottom fillers, buffer coating materials, copper-clad laminates, flexible substrates, high-frequency device modules, antenna modules, and vehicle-mounted radars. In addition, bonding sheets refer to, in the case of manufacturing a multilayer printed wiring substrate, an insulating adhesive layer forming material for bonding a conductor layer to an organic insulating layer.
[0093] Furthermore, the hollow particles of the present invention, when added to a molded body, have excellent effects as a lightweight material, heat insulating material, sound insulating material, shockproof material, etc., and are therefore suitable as an additive for a molded body. For example, they can be used as an additive for a resin molded body. Furthermore, they can also be contained as a filler in a fiber-reinforced molded body formed using a resin and reinforcing fibers.
[0094] In addition, the hollow particles of the present invention have high porosity, are not easily broken, and have excellent heat resistance, so they meet the heat insulation and cushioning properties (shock absorption (cushion) properties) required by the primer material, and also meet the heat resistance for thermal paper applications. In addition, the hollow particles of the present invention are also useful as plastic pigments with excellent gloss, hiding power, etc.
[0095] Furthermore, the hollow particles of the present invention can contain useful components such as fragrances, chemicals, pesticides, and ink components by methods such as impregnation treatment, reduced pressure or pressurized impregnation treatment, and can therefore be used for various purposes depending on the components contained therein.
[0096] The hollow particles of the present invention are also suitable for use as rust preventives. The hollow particles of the present invention are also useful as additives for reducing electrical conductivity, and therefore, for example, a coating containing the hollow particles of the present invention can be used as an anti-rust coating (coating base, lubricating coating, etc.) for improving the corrosion resistance and rust resistance of steel materials, etc. In addition, the hollow particles added to the anti-rust coating can also contain an anti-rust additive.
[0097] <Method for producing hollow particles>
[0098] The hollow particles of the present invention can be preferably produced by a production method comprising the following (A) mixed solution preparation step, (B) suspension step, (C) polymerization step, and (D) solvent removal step.
[0099] That is, the hollow particles of the present invention can be preferably produced by a production method comprising the following steps:
[0100] (A) a mixed solution preparation step of preparing a mixed solution containing a polymerizable monomer including a cross-linkable monomer, a hydrophobic organic solvent, a polymerization initiator, and an aqueous medium;
[0101] (B) a suspension step of suspending the mixed solution obtained in the mixed solution preparation step to prepare a suspension in which droplets of a polymerizable monomer composition containing a polymerizable monomer, a hydrophobic organic solvent and a polymerization initiator are dispersed in an aqueous medium;
[0102] (C) a polymerization step of subjecting the suspension obtained in the suspending step to a polymerization reaction to prepare a precursor composition containing precursor particles having a hollow portion and enclosing a hydrophobic organic solvent in the hollow portion; and
[0103] (D) A solvent removal step of removing the hydrophobic organic solvent contained in the precursor particles obtained in the polymerization step.
[0104] (A) Mixed solution preparation process
[0105] The mixed solution preparation step is a step of preparing a mixed solution containing a polymerizable monomer including a crosslinkable monomer, a hydrophobic organic solvent, a polymerization initiator, and an aqueous medium. The hollow particles of the present invention are preferably produced by a production method including such a step.
[0106] [Polymerizable monomer]
[0107] As the polymerizable monomer, the above-mentioned crosslinkable monomer and, if necessary, the above-mentioned monofunctional monomer are used. The monomer composition of the polymerizable monomer may be any monomer composition as long as the monomer composition of the target shell polymer can be obtained.
[0108] The content of the polymerizable monomer (the total amount of the cross-linking monomer and the monofunctional monomer) in the mixed solution prepared in the mixed solution preparation step is not particularly limited, but is preferably 15 to 55% by mass, more preferably 25 to 50% by mass, relative to 100% by mass of the total mass of the components in the mixed solution excluding the aqueous medium.
[0109] [Hydrophobic organic solvent]
[0110] As the hydrophobic organic solvent, a non-polymerizable organic solvent that is poorly soluble in water is used. The hydrophobic organic solvent functions as a spacer that forms a hollow portion inside the particle.
[0111] The hydrophobic organic solvent is not particularly limited, and hydrocarbon solvents can be preferably used. Specific examples thereof include: saturated hydrocarbon solvents such as butane, pentane, n-hexane, cyclohexane, heptane, octane, etc.; aromatic hydrocarbon solvents such as benzene, toluene, xylene, etc.; and highly volatile solvents such as carbon disulfide and carbon tetrachloride.
[0112] As a hydrophobic organic solvent, the proportion of saturated hydrocarbon solvents is preferably 50% by mass or more in the total amount of 100% by mass of the hydrophobic organic solvent. As a result, phase separation occurs sufficiently in the droplets of the polymerizable monomer composition prepared in the suspension step described later, so that hollow particles having only one hollow portion can be easily obtained and the generation of porous particles can be suppressed. From the viewpoint of further suppressing the generation of porous particles and the viewpoint that the hollow portion of each hollow particle is easy to become uniform, the proportion of saturated hydrocarbon solvents is preferably 60% by mass or more, and more preferably 80% by mass or more in the total amount of 100% by mass of the hydrophobic organic solvent.
[0113] In addition, as the hydrophobic organic solvent, a hydrocarbon solvent having 5 to 8 carbon atoms is preferred. A hydrocarbon solvent having 5 to 8 carbon atoms is easily included in the precursor particles during the polymerization step described later, and can be easily removed from the precursor particles during the solvent removal step described later. Among them, a hydrocarbon solvent having 6 to 8 carbon atoms is particularly preferred.
[0114] In addition, as the hydrophobic organic solvent, from the viewpoint of easy removal in the solvent removal step described later, a hydrophobic organic solvent having a boiling point of less than 130°C is preferred, and a hydrophobic organic solvent having a boiling point of less than 115°C is more preferred. On the other hand, from the viewpoint of easy inclusion in the precursor particles, a hydrophobic organic solvent having a boiling point of more than 30°C is preferred, and a hydrophobic organic solvent having a boiling point of more than 50°C is more preferred.
[0115] When the hydrophobic organic solvent is a mixed solvent containing a plurality of hydrophobic organic solvents and has a plurality of boiling points, the boiling point of the hydrophobic organic solvent refers to the boiling point of the solvent with the highest boiling point among the solvents contained in the mixed solvent, that is, the highest boiling point among the plurality of boiling points.
[0116] In addition, the hydrophobic organic solvent preferably has a relative dielectric constant of 3 or less at 20°C. The relative dielectric constant is one of the indicators indicating the polarity of a compound. It is considered that when the relative dielectric constant of the hydrophobic organic solvent is sufficiently small to be 3 or less, phase separation in the droplets of the polymerizable monomer composition prepared in the suspension step described later proceeds rapidly, and a hollow portion is easily formed.
[0117] Examples of hydrophobic organic solvents having a relative dielectric constant of 3 or less at 20°C include heptane (1.9), cyclohexane (2.0), benzene (2.3), toluene (2.4), etc. (the relative dielectric constant values are in parentheses). Regarding the relative dielectric constant at 20°C, reference can be made to the values and other technical information recorded in known literature (e.g., The Basics of Chemical Handbook, edited by the Chemical Society of Japan, revised 4th edition, Maruzen Co., Ltd., published on September 30, 1996, pages II-498 to II-503). As a method for measuring the relative dielectric constant at 20°C, for example, a relative dielectric constant test performed in accordance with 23 of JISC 2101:1999 with the measuring temperature set to 20°C can be cited.
[0118] The content of the hydrophobic organic solvent in the mixed liquid is preferably 50 to 500 parts by mass, more preferably 60 to 400 parts by mass, further preferably 80 to 350 parts by mass, particularly preferably 100 to 300 parts by mass, based on 100 parts by mass of the total mass of the polymerizable monomers.
[0119] [Polymerization initiator]
[0120] As the polymerization initiator, an oil-soluble polymerization initiator is preferably used. By using an oil-soluble polymerization initiator as the polymerization initiator, the polymerization initiator can be appropriately introduced into the liquid droplets of the polymerizable monomer composition in the suspension obtained in the suspension step described below.
[0121] The oil-soluble polymerization initiator is not particularly limited as long as it is a lipophilic polymerization initiator having a solubility in water of 0.2 mass % or less. Examples of the oil-soluble polymerization initiator include benzoyl peroxide, lauroyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxydiethylacetate, tert-butyl peroxypivalate, 2,2'-azobis(2,4-dimethylvaleronitrile), and azobisisobutyronitrile.
[0122] The content of the polymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, and further preferably 0.5 to 3 parts by mass relative to 100 parts by mass of the total mass of the polymerizable monomer in the mixed solution. By making the content of the polymerization initiator within the above range, the polymerization reaction is fully carried out, and the possibility of residual polymerization initiator after the polymerization reaction is completed is small, and in addition, the possibility of carrying out unexpected side reactions is also small.
[0123] [Water-based media]
[0124] Examples of the aqueous medium include a medium selected from water, a hydrophilic solvent, and a mixture of water and a hydrophilic solvent.
[0125] The hydrophilic solvent is not particularly limited as long as it is a hydrophilic solvent that is sufficiently miscible with water without phase separation, and examples thereof include alcohols such as methanol and ethanol; tetrahydrofuran (THF); and dimethyl sulfoxide (DMSO).
[0126] Among aqueous media, water is preferably used from the perspective of polarity. When a mixture of water and a hydrophilic solvent is used, it is preferred that the polarity of the mixture as a whole does not become too low from the perspective of appropriately forming droplets of a polymerizable monomer composition containing a polymerizable monomer, a hydrophobic organic solvent, and a polymerization initiator. When a mixture of water and a hydrophilic solvent is used, the mixing ratio (mass ratio) of water and the hydrophilic solvent is preferably set to water:hydrophilic solvent = 99:1 to 50:50.
[0127] In addition, in the mixed solution preparation process, in addition to using polymerizable monomers, hydrophobic organic solvents, polymerization initiators and aqueous media, a dispersion stabilizer is also preferably used. That is, the mixed solution preparation process is preferably a process for preparing a mixed solution containing polymerizable monomers, hydrophobic organic solvents, polymerization initiators, aqueous media and dispersion stabilizers.
[0128] The dispersion stabilizer is a compound that disperses the droplets of the polymerizable monomer composition in the aqueous medium in the suspension step described below, and may be either an inorganic dispersion stabilizer or an organic dispersion stabilizer.
[0129] Examples of the inorganic dispersion stabilizer include colloidal silica, magnesium hydroxide, calcium phosphate, calcium carbonate, barium sulfate, calcium oxalate, calcium carbonate, magnesium carbonate, barium carbonate, tricalcium phosphate, aluminum hydroxide, magnesium hydroxide, iron hydroxide, hydroxyapatite, diatomaceous earth silicate, clay, and bentonite.
[0130] Examples of the organic dispersion stabilizer include methyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, and starch.
[0131] Among these, inorganic dispersion stabilizers are preferred from the viewpoint of high dispersion stabilization effect and easier control of the particle size of droplets of the polymerizable monomer composition containing polymerizable monomers, hydrophobic organic solvents and polymerization initiators. Among inorganic dispersion stabilizers, metal-containing dispersion stabilizers are preferred, and inorganic metal salts that are sparingly soluble in water are more preferred. In addition, as sparingly soluble inorganic metal salts, inorganic metal salts having a solubility of 0.5 g or less in 100 g of water are preferred, and examples thereof include magnesium hydroxide, calcium hydroxide, barium hydroxide, calcium phosphate, etc., and magnesium hydroxide is more preferred among these. Dispersion stabilizers can be used alone or in combination of two or more.
[0132] In addition, from the viewpoint of further improving the dispersion stabilization effect, the dispersion stabilizer is preferably used in the form of a dispersion or solution of the dispersion stabilizer by dispersing or dissolving in an aqueous medium. That is, in the mixed solution preparation process, the mixed solution is preferably obtained by mixing the dispersion stabilizer in the form of a dispersion or solution with a polymerizable monomer, a hydrophobic organic solvent and a polymerization initiator. In addition, as the aqueous medium, the above-mentioned aqueous medium can be used.
[0133] The mixing ratio of the dispersion stabilizer to the aqueous medium in the dispersion or solution of the dispersion stabilizer is preferably 0.7:100 to 7:100, more preferably 1.0:100 to 4.0:100, and even more preferably 1.4:100 to 3:100 in terms of the mass ratio of "dispersion stabilizer: aqueous medium". By setting the mixing ratio of the dispersion stabilizer to the aqueous medium within the above range, the dispersion stabilization effect can be more appropriately improved.
[0134] As a method for preparing a dispersion or solution of a dispersion stabilizer, a method of directly mixing the dispersion stabilizer with an aqueous medium can be adopted. Preferably, a method of generating the dispersion stabilizer by mixing two or more compounds serving as precursors of the dispersion stabilizer (i.e., two or more precursor compounds) in an aqueous medium and reacting them is adopted.
[0135] In addition, the precursor compound used when mixing two or more precursor compounds in an aqueous medium is not particularly limited. For example, when a hydroxide salt that is poorly soluble in water, such as magnesium hydroxide, calcium hydroxide, or barium hydroxide, is used as a dispersion stabilizer, the two or more precursor compounds include a combination of a water-soluble polyvalent metal salt and an alkali metal hydroxide.
[0136] As water-soluble polyvalent metal salts, hydrochlorides, sulfates, nitrates, acetates, etc. of polyvalent metals such as magnesium, calcium, aluminum, iron, copper, manganese, nickel, and tin can be cited. Among these, water-soluble salts of magnesium and calcium are preferred. In addition, as alkali metal hydroxides, sodium hydroxide, potassium hydroxide, lithium hydroxide, etc. can be cited. For example, when magnesium hydroxide is used as a dispersion stabilizer, as two or more precursor compounds, a combination of magnesium chloride and sodium hydroxide is preferred.
[0137] The method for mixing two or more precursor compounds in an aqueous medium is not particularly limited. When a combination of a water-soluble polyvalent metal salt and an alkali metal hydroxide is prepared, a method in which an aqueous medium solution of an alkali metal hydroxide is added dropwise to an aqueous medium solution of a water-soluble polyvalent metal salt under stirring is preferred.
[0138] In the aqueous medium solution of the water-soluble multivalent metal salt, the content of the water-soluble multivalent metal salt is preferably 2 to 8 parts by weight, more preferably 3 to 6 parts by weight relative to 100 parts by weight of the aqueous medium solution. In addition, in the aqueous medium solution of the alkali metal hydroxide, the content of the alkali metal hydroxide is preferably 6 to 20 parts by weight, more preferably 8 to 18 parts by weight relative to 100 parts by weight of the aqueous medium solution. In addition, as the aqueous medium, the above-mentioned aqueous medium can be used.
[0139] In the mixed solution preparation process, the mixed solution can be obtained by mixing the above-mentioned components by stirring or the like. At this time, in addition to the above-mentioned components, other materials can also be mixed as needed. In the mixed solution preparation process, a mixed solution is prepared in which an oil phase containing lipophilic materials such as a polymerizable monomer, a hydrophobic organic solvent and a polymerization initiator is dispersed in a water phase containing an aqueous medium and a dispersion stabilizer used as needed in a particle size of several millimeters. The dispersion state of these components in the mixed solution can also be observed by the naked eye according to the type of each component.
[0140] Furthermore, in the mixed solution preparation step, from the viewpoint of making the composition of the shell portion more uniform, it is preferred to prepare in advance an oil phase containing a polymerizable monomer, a hydrophobic organic solvent and a polymerization initiator, and to mix it with a dispersion or solution in which a dispersion stabilizer is dispersed or dissolved in an aqueous medium, thereby preparing the mixed solution.
[0141] (B) Suspension process
[0142] The suspending step is a step of preparing a suspension in which droplets of a polymerizable monomer composition containing a polymerizable monomer, a hydrophobic organic solvent and a polymerization initiator are dispersed in an aqueous medium by suspending the mixed solution obtained in the mixed solution preparing step.
[0143] The suspension method for forming the droplets of the polymerizable monomer composition is not particularly limited, and a method of using a stirring device capable of strong stirring to stir the mixed solution obtained in the above-mentioned mixed solution preparation process is preferred. As the stirring device used in the suspension process, there is no particular limitation, and for example, a stirring device having a stirring blade or a rotor and a supply tank for supplying to the stirring machine can be used. In addition, as a stirring machine, as long as it has a stirring blade or a rotor, it is not particularly limited. From the viewpoint of being able to efficiently form a suspension, the following stirring machine is preferred: a combination of a rotor and a stator having comb-tooth-shaped concentric rings, the rotor is rotated at high speed, the above-mentioned dispersion is circulated from the inside of the rotor to the outside of the stator, and the dispersion is stirred in the gap between the rotor and the stator.
[0144] Examples of a stirrer having such a structure include an in-line emulsifying and dispersing machine. Examples of the in-line emulsifying and dispersing machine include the product name "Cavitron" (manufactured by Eurotec Co., Ltd.), the product name "Milder" (manufactured by Pacific Machinery Co., Ltd.), the product name "EBARA MILDER" (manufactured by EBARA MISSION CO., LTD.), the product name "TK Pipeline Homomixer" (manufactured by Tokushu Kikka Kogyo Co., Ltd.), the product name "Colloid Mill" (manufactured by Kobelco Pan-Techno Co., Ltd.), the product name "Slacher" (manufactured by Nippon Coking Industry Co., Ltd.), the product name "Trigonal Wet Type Fine Pulverizer" (manufactured by Mitsui Miike Chemical Industry Co., Ltd.), and the product name "Fine Flow Mill" (manufactured by Pacific Machinery Co., Ltd.).
[0145] In the suspension step, a suspension in which droplets of the polymerizable monomer composition containing the above-mentioned lipophilic material are uniformly dispersed in an aqueous medium can be obtained as a suspension. Such droplets of the polymerizable monomer composition are difficult to observe with the naked eye, but can be observed by a known observation device such as an optical microscope. In addition, in the suspension step, phase separation occurs in the droplets of the polymerizable monomer composition, so the hydrophobic organic solvent with low polarity becomes easy to gather inside the droplets. As a result, in the obtained droplets, the hydrophobic organic solvent is distributed inside, and the material other than the hydrophobic organic solvent is distributed on the periphery.
[0146] (C) Polymerization process
[0147] The polymerization step is a step of subjecting the suspension prepared in the above-mentioned suspending step to a polymerization reaction to prepare a precursor composition having a hollow portion and enclosing a hydrophobic organic solvent in the hollow portion.
[0148] In the polymerization step, the polymerizable monomer in the droplets of the polymerizable monomer composition is polymerized while the droplets contain the hydrophobic organic solvent, thereby forming precursor particles having a shell of a resin containing a polymer of the polymerizable monomer and a hollow portion filled with the hydrophobic organic solvent.
[0149] In the polymerization process, the droplets of the polymerizable monomer composition are provided to the polymerization reaction in a state of enclosing the hydrophobic organic solvent, thereby making it easy to carry out the polymerization reaction while maintaining the shape, and to adjust the size and porosity of the precursor particles. In addition, since the polymerizable monomer and the hydrophobic organic solvent are used in combination, and since the hydrophobic organic solvent has a low polarity relative to the shell of the precursor particles, the hydrophobic organic solvent is not easy to merge with the shell, so phase separation occurs sufficiently, and it is easy to form only one hollow portion.
[0150] The polymerization method is not particularly limited, and examples thereof include batch method (intermittent method), semi-continuous method, continuous method, etc. The polymerization temperature is preferably 40 to 90° C., more preferably 50 to 80° C. The polymerization reaction time is preferably 1 to 48 hours, more preferably 3 to 24 hours.
[0151] Through the polymerization step, a precursor composition is obtained in which the precursor particles containing the hydrophobic solvent are dispersed in the aqueous phase mainly composed of the aqueous medium.
[0152] (D) Solvent Removal Step
[0153] The solvent removal step is a step of removing the hydrophobic organic solvent contained in the precursor particles obtained in the polymerization step.
[0154] Before the solvent is removed by the solvent removal process, the precursor composition obtained by the polymerization process is preferably subjected to solid-liquid separation in advance, and a solid component comprising precursor particles is obtained by solid-liquid separation, wherein the precursor particles contain a hydrophobic organic solvent. After the solid component comprising the precursor particles is obtained by solid-liquid separation, the hydrophobic organic solvent contained in the precursor particles can be removed in the gas, and the hydrophobic organic solvent inside the precursor particles is replaced by air to obtain hollow particles filled with gas.
[0155] The method of solid-liquid separation of the precursor composition is not particularly limited, and known methods can be used. As the method of solid-liquid separation, for example, centrifugation, filtration, static separation, etc. can be mentioned. Among these, centrifugation or filtration can be used. From the viewpoint of simplicity of operation, centrifugation can be used. After solid-liquid separation, any process such as pre-drying process can be further used. As the pre-drying process, for example, a process in which the solid component obtained after the solid-liquid separation process is pre-dried by drying appliances such as drying devices such as driers and hand dryers can be mentioned.
[0156] In addition, the "in gas" in the solvent removal process strictly refers to an environment in which there is no liquid component at all outside the precursor particles and an environment in which there is only a very small amount of liquid component outside the precursor particles that does not affect the removal of the hydrophobic organic solvent. The so-called "in gas" can be changed to a state in which the precursor particles are not present in the slurry, and can also be changed to a state in which the precursor particles are present in the dry powder. That is, in the solvent removal process, it is desired that the precursor particles remove the hydrophobic organic solvent in an environment in which they are in direct contact with the external gas.
[0157] The method for removing the hydrophobic organic solvent in the precursor particles in the gas is not particularly limited, and a known method can be used, such as reduced pressure drying method, heating drying method, airflow drying method, and these methods can also be used in combination. In particular, when using the heating drying method, the heating temperature needs to be above the boiling point of the hydrophobic organic solvent and below the maximum temperature at which the shell structure of the precursor particles is not damaged. Therefore, according to the composition of the shell in the precursor particles and the type of the hydrophobic organic solvent, the heating temperature is preferably 50 to 200 ° C, more preferably 70 to 200 ° C, and further preferably 100 to 200 ° C. By the drying operation in the gas, the hydrophobic organic solvent inside the precursor particles is replaced by the external gas, and the result is to obtain hollow particles in which the gas occupies the hollow part.
[0158] Drying environment is not particularly limited and can be appropriately selected according to the purpose of the hollow particle. As drying environment, for example, air, oxygen, nitrogen, argon, etc. can be considered. In addition, after the inside of the hollow particle is temporarily filled with gas, reduced pressure drying is carried out, thus, the hollow particle that is temporarily vacuum inside can also be obtained.
[0159] In addition, the slurry-like precursor composition obtained in the polymerization process may not be subjected to solid-liquid separation, but in the slurry comprising precursor particles and an aqueous medium, the hydrophobic organic solvent contained in the precursor particles is replaced with the aqueous medium of the slurry, thereby removing the hydrophobic organic solvent. In this method, an inert gas is blown into the precursor composition at a temperature above the temperature of 35 ° C minus the boiling point of the hydrophobic organic solvent, and the hydrophobic organic solvent contained in the precursor particles in the precursor composition is removed, thereby reducing the residual amount of the hydrophobic organic solvent in the hollow particles. Here, when the hydrophobic organic solvent is a mixed solvent containing a plurality of hydrophobic organic solvents and having a plurality of boiling points, the boiling point of the hydrophobic organic solvent in the solvent removal process refers to the boiling point of the solvent with the highest boiling point in the solvent contained in the mixed solvent, that is, the highest boiling point among the plurality of boiling points.
[0160] From the viewpoint of reducing the residual amount of the hydrophobic organic solvent in the hollow particles, the temperature when the inert gas is blown into the above-mentioned precursor composition is preferably a temperature above the temperature at which 30°C is subtracted from the boiling point of the hydrophobic organic solvent, and more preferably a temperature above the temperature at which 20°C is subtracted from the boiling point of the hydrophobic organic solvent. In addition, the temperature during the blowing is usually a temperature above the polymerization temperature in the above-mentioned polymerization step. Although not particularly limited, the temperature during the blowing can be made 50°C or more and 100°C or less. The inert gas blown is not particularly limited, and examples thereof include nitrogen, argon, etc.
[0161] The conditions of the gas blowing can be appropriately adjusted according to the type and amount of the hydrophobic organic solvent so that the hydrophobic organic solvent contained in the precursor particles can be removed. There are no particular limitations on the conditions, for example, a method of blowing inert gas for 1 to 10 hours at an amount of 1 to 3 L / min is preferred. According to this method, an aqueous slurry containing an aqueous medium in the precursor particles can be obtained. The hollow particles obtained by solid-liquid separation of the slurry are dried to remove the aqueous medium in the hollow particles, thereby obtaining hollow particles in which the gas occupies the hollow portion.
[0162] Compared with a method in which a slurry-like precursor composition is subjected to solid-liquid separation and then the hydrophobic organic solvent in the precursor particles is removed in a gas to obtain hollow particles whose hollow portions are filled with gas, and a slurry containing precursor particles and an aqueous medium is prepared by replacing the hydrophobic organic solvent contained in the precursor particles with the aqueous medium of the slurry, followed by solid-liquid separation and then removing the aqueous medium in the precursor particles in a gas to obtain hollow particles whose hollow portions are filled with gas, the former method has the advantage that the hollow particles are not easily broken in the step of removing the hydrophobic organic solvent, and the latter method has the advantage that the residual hydrophobic organic solvent is reduced by blowing with an inert gas.
[0163] In addition, as a method for removing the hydrophobic organic solvent contained in the precursor particles without performing solid-liquid separation on the slurry-like precursor composition obtained in the polymerization step after the polymerization step and before the solid-liquid separation step, for example: a method of evaporating the hydrophobic organic solvent contained in the precursor particles from the precursor composition under a specified pressure (high pressure, normal pressure or reduced pressure); a method of introducing an inert gas such as nitrogen, argon, helium or water vapor into the precursor composition under a specified pressure (high pressure, normal pressure or reduced pressure) to remove the hydrophobic organic solvent by distillation.
[0164] (E) Other processes
[0165] The above-mentioned production method may include other steps. Examples of other steps include (E-1) a cleaning step and (E-2) a hollow portion re-replacing step.
[0166] (E-1) Cleaning process
[0167] The above-mentioned manufacturing method preferably includes a cleaning process before or after the recovery process. For example, when a dispersion stabilizer is used, in order to remove the dispersion stabilizer remaining in the hollow particle slurry containing hollow particles and an aqueous medium before the recovery process, a cleaning process for cleaning by adding an acid or an alkali is preferably included. When the dispersion stabilizer used is an acid-soluble dispersion stabilizer, it is preferably cleaned by adding an acid to a precursor composition containing precursor particles. On the other hand, when the dispersion stabilizer used is an alkali-soluble dispersion stabilizer, it is preferably cleaned by adding an alkali to a precursor composition containing precursor particles.
[0168] When an acid-soluble dispersion stabilizer is used as the dispersion stabilizer, an acid is added to the precursor composition containing the precursor particles to adjust the pH to preferably 6.5 or less, and more preferably to 6 or less. As the acid to be added, inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as formic acid and acetic acid can be used, and sulfuric acid is particularly preferred from the viewpoint of high removal efficiency of the dispersion stabilizer and small burden on the production equipment.
[0169] (E-2) Hollow portion replacement step
[0170] The re-replacement process of the hollow part refers to the process of replacing the gas or liquid inside the hollow particle with other gas or liquid. By such replacement, the environment inside the hollow particle can be changed, or molecules can be selectively enclosed inside the hollow particle, or the chemical structure inside the hollow particle can be modified according to the application.
[0171] <Resin composition>
[0172] The hollow particles of the present invention can be mixed with a resin to form a resin composition.
[0173] The resin composition may be a liquid resin composition or a resin molded body. Examples of the liquid resin composition include: a liquid resin composition containing a liquid matrix resin before the curing reaction; a liquid resin composition obtained by dissolving or dispersing each component in a solvent; or a liquid resin composition in which the matrix resin is a thermoplastic resin and the resin composition is made liquid by melting the resin. Examples of the resin molded body include, for example, a resin molded body obtained by molding the above-mentioned liquid resin composition by a known method.
[0174] The matrix resin contained in the resin composition is not particularly limited, and may be, for example, a thermosetting resin or a thermoplastic resin. In addition, the resin contained in the resin composition may be an unreacted monomer, a prepolymer or a macromonomer, a polymer, or a precursor of a curing resin such as polyamic acid. The matrix resin contained in the resin composition may contain a thermoplastic elastomer as a resin. Furthermore, the resin composition may also contain rubber.
[0175] As the thermosetting resin, known thermosetting resins can be used without particular limitation, and examples thereof include phenolic resins, melamine resins, urea resins, unsaturated polyester resins, epoxy resins, polyurethane resins, silicone resins, alkyd resins, thermosetting modified polyphenylene ether resins, thermosetting polyimide resins, benzophenone resins, and the like. Oxazine resins, urea-formaldehyde resins, allyl resins, aniline resins, maleimide resins, bismaleimide triazine resins, liquid crystalline polyester resins, vinyl ester resins, unsaturated polyester resins, cyanate resins, polyetherimide resins, etc. These thermosetting resins can be used alone or in combination of two or more.
[0176] The thermoplastic resin is not particularly limited, and known thermoplastic resins can be used, for example: polyolefins such as polypropylene and polyethylene; polyamides such as PA6, PA66, and PA12; polyimide, polyamide-imide, polyetherimide, polyetherketoneketone, polyvinyl chloride, polystyrene, poly(meth)acrylate, polycarbonate, polyvinylidene fluoride, acrylonitrile-butadiene-styrene copolymer (ABS), acrylonitrile-styrene copolymer (AS), polyphenylene ether, polyphenylene sulfide, polyester, polytetrafluoroethylene, thermoplastic elastomer, etc. These thermoplastic resins can be used alone or in combination of two or more.
[0177] In applications requiring a low dielectric constant or a low dielectric loss tangent, epoxy resins, thermosetting modified polyphenylene ether resins, thermosetting polyimide resins, silicone resins, benzophenone resins, and the like are particularly preferred as resins. Insulating resins such as oxazine resins, melamine resins, urea-formaldehyde resins, allyl resins, phenolic resins, unsaturated polyester resins, polyurethane resins, and aniline resins are preferably used, and epoxy resins, thermosetting polyimide resins, modified polyphenylene ether resins, silicone resins, benzophenone resins, and the like are particularly preferred. Oxazine-based resins and melamine-based resins, etc. These insulating resins can be used alone or in combination of two or more.
[0178] As the thermoplastic elastomer, a thermoplastic elastic polymer that has been used as a molding resin in the past can be used, and examples thereof include urethane elastomers, styrene elastomers, olefin elastomers, amide elastomers, and ester elastomers. Thermoplastic elastomers are materials that generally exhibit rubber elasticity at room temperature (25° C.) and have the property of being plasticized and molded at high temperatures. Thermoplastic elastomers can be used alone or in combination of two or more.
[0179] The rubber may include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), ethylene-propylene-diene terpolymer (EPDM), etc. The rubber may be used alone or in combination of two or more.
[0180] In all solid components of 100% by mass of resin combination, the content of resin is not particularly limited, and is preferably below 50 to 95% by mass. By making the content of resin more than the above-mentioned lower limit, the moldability when making a resin molded body is excellent, and the mechanical strength of the resin molded body obtained is excellent. On the other hand, by making the content of resin below the above-mentioned upper limit, the hollow particles of the present invention can be fully contained, so the effects such as lightweight, low dielectric loss tangent brought by the hollow particles of the present invention can be fully exerted.
[0181] The resin composition may further contain additives such as a curing agent, a curing catalyst or an initiator for curing the resin, depending on the type of resin. Examples of the curing agent include amines, acid anhydrides, imidazoles, thiols, phenols, naphthols, benzophenones, and the like. Oxidase, cyanate, carbodiimide, etc. The content of the curing agent is not particularly limited, and may be, for example, 5 to 120 parts by mass relative to 100 parts by mass of the resin.
[0182] In the total solid components of 100 mass % of resin combination, the content of hollow particles of the present invention is not particularly limited, and is preferably 5~50 mass %. By making the content of hollow particles be more than the above-mentioned lower limit, the effects such as lightweight, low dielectric loss tangent brought by the hollow particles of the present invention can be fully exerted. On the other hand, by making the content of hollow particles be below the above-mentioned upper limit, resin can be fully contained, therefore formability and mechanical strength can be improved.
[0183] As long as the effects of the present invention are not impaired, the resin composition may further contain additives such as a compatibilizer, an ultraviolet absorber, a colorant, a heat stabilizer, a filler, a solvent, etc. as needed. In addition, the resin composition may further contain organic or inorganic fibers such as carbon fiber, glass fiber, aramid fiber, polyethylene fiber, etc.
[0184] The resin composition can be obtained by, for example, mixing the hollow particles of the present invention, the resin, and the additives, solvents, etc. further added as required. When the resin in the resin composition is a thermoplastic resin, the hollow particles of the present invention and the additives further added as required can be added to the molten thermoplastic resin and melt-kneaded to mix. The resin composition thus obtained can be a liquid resin composition, or the resin composition can be a resin molded body made of a liquid resin composition by a known method.
[0185] The method for manufacturing the resin molded body is not particularly limited. For example, the resin molded body can be obtained by the following method: a liquid resin composition in which a liquid matrix resin before the curing reaction contains hollow particles, or a liquid resin composition in which each component is dissolved or dispersed in a solvent is applied to a support, and dried and cured as needed.
[0186] Examples of the material of the support include resins such as polyethylene terephthalate and polyethylene naphthalate, and metals such as copper, aluminum, nickel, chromium, gold, and silver. These supports may be coated with a release agent on their surfaces.
[0187] In addition, it is also possible to obtain a resin molded body by impregnating the liquid resin composition in the substrate and drying and curing as required. As the above-mentioned substrate, inorganic fibers such as carbon fiber, glass fiber, metal fiber, ceramic fiber, and organic synthetic fibers such as polyamide fiber, polyester fiber, polyolefin fiber, and Novoloid fiber can be cited, especially preferably glass fiber (glass cloth). In addition, the form of the above-mentioned substrate is not limited, and fabrics, nonwoven fabrics, etc. can be used.
[0188] As a method for applying the liquid resin composition, a known method can be used, and examples thereof include a dip coating method, a roll coating method, a curtain coating method, a die coating method, a slit coating method, and a gravure coating method.
[0189] When the liquid resin composition contains a solvent, it is preferred to dry the resin composition after the above-mentioned coating or impregnation. The drying temperature is preferably set to a temperature at which the matrix resin does not solidify, usually 20°C or more and 200°C or less, preferably 30°C or more and 150°C or less. In addition, the drying time is usually 30 seconds or more and 1 hour or less, preferably 1 minute or more and 30 minutes or less.
[0190] The curing reaction of the resin composition is carried out by a method corresponding to the type of resin, without particular limitation. In the case of a resin that is cured by heating, the temperature of the heating for the curing reaction can be appropriately adjusted according to the type of resin, without particular limitation, and is usually above 30°C and below 400°C, preferably above 70°C and below 300°C, and more preferably above 100°C and below 200°C. In addition, the curing time is above 5 minutes and below 5 hours, preferably above 30 minutes and below 3 hours. The heating method is not particularly limited, for example, it can be carried out using an electric oven.
[0191] In addition, the liquid resin before the curing reaction and the resin dissolved or dispersed in the solvent may be a thermosetting resin or a thermoplastic resin.
[0192] Alternatively, a resin molded body may be obtained by molding a liquid resin composition containing a thermoplastic resin as a resin and melted into a desired shape by a known molding method such as extrusion molding, injection molding, press molding, or compression molding.
[0193] The shape of the resin molding is not particularly limited, and various shapes that can be molded can be made, such as sheet, film, plate, tubular and other various three-dimensional shapes. In addition, when the resin molding includes fibers, the fibers in the resin molding can be nonwoven. In addition, when the resin molding includes fibers, it can also be a molding of a resin composition having hollow particles of the present invention added to a fiber-reinforced plastic containing the above-mentioned resin and fibers.
[0194] Examples of the application of the resin composition of the present invention include applications in which the resin composition can be used in the applications of the hollow particles of the present invention described above.
[0195] Example
[0196] Hereinafter, the present invention will be further specifically described by way of examples and comparative examples, but the present invention is not limited to these examples. In addition, parts and % are by weight unless otherwise specified. Various measurements were performed according to the following methods.
[0197] <True density and porosity of hollow particles>
[0198] (Determination of Apparent Density of Hollow Particles)
[0199] First, in a volume of 100cm 3 Fill the volumetric flask to about 30 cm 3 The mass of the hollow particles was accurately weighed. Next, the volumetric flask filled with the hollow particles was filled with isopropyl alcohol to the mark while being careful not to mix in bubbles. The mass of isopropyl alcohol added to the volumetric flask was accurately weighed, and the apparent density D of the hollow particles was calculated based on the following formula (II): 1 (g / cm 3 ).
[0200] The apparent density of hollow particles is D 1 (g / cm 3 ) = [mass of hollow particles] ÷ (100 - [mass of isopropyl alcohol] ÷ [density of isopropyl alcohol at the measurement temperature]) (II)
[0201] (Determination of true density of hollow particles)
[0202] After the hollow particles are crushed in advance, the volume is 100cm 3 A volumetric flask is filled with about 10 g of hollow particle fragments, and the mass of the filled fragments is accurately weighed. Next, isopropyl alcohol is added to the volumetric flask in the same manner as the above-mentioned apparent density measurement, and the mass of isopropyl alcohol is accurately weighed. The true density D of the hollow particles is calculated based on the following formula (I): 0 (g / cm 3 ).
[0203] Hollow particle true density D 0 (g / cm 3 ) = [mass of the hollow particle fragments] ÷ (100 - [mass of isopropyl alcohol] ÷ [density of isopropyl alcohol at the measurement temperature]) (I)
[0204] (Calculation of the porosity of hollow particles)
[0205] The porosity (%) of the hollow particles is calculated based on the apparent density D of the hollow particles. 1 and true density D 0 It is calculated by the following formula (III).
[0206] Porosity of hollow particles (%) = 100 - [apparent density of hollow particles D1 ]÷[True density of hollow particles D 0 ]×100 (III)
[0207] <Volume average particle size (Dv) and particle size distribution (Dv / Dn) of hollow particles>
[0208] The volume average particle size (Dv) and number average particle size (Dn) of the hollow particles were measured using a particle size distribution measuring machine (manufactured by Beckman Coulter, product name: Multisizer 4e), and the particle size distribution (Dv / Dn) was calculated. The measurement conditions were set as pore size: 50 μm, dispersion medium: ISOTON II (product name), concentration 10%, and number of particles measured: 100,000. Specifically, 0.2 g of the hollow particles were taken into a beaker, and a surfactant aqueous solution (manufactured by Fujifilm Corporation, product name: DRIWEL) as a dispersant was added thereto. 2 ml of the dispersion medium was further added thereto to wet the hollow particles, and then 10 ml of the dispersion medium was added, and after dispersing them for 1 minute using an ultrasonic disperser, the measurement was performed using the above-mentioned particle size distribution measuring machine.
[0209] <Toluene immersion test>
[0210] Under the environment of 25 ℃, 0.1 mg of hollow particles were added to 4 mL of toluene, and the mixture was shaken for 10 minutes at a shaking speed of 100 rpm using an oscillator. After the shaken mixture was left to stand for 48 hours or 120 hours, the hollow particles precipitated in toluene were separated by a centrifuge, dried, and the mass of the hollow particles precipitated in toluene was measured. Then, the ratio of the mass of the hollow particles precipitated in toluene to the mass of the entire hollow particles immersed in toluene was calculated, and the ratio of the precipitated hollow particles was obtained, and the evaluation was performed based on the following evaluation criteria.
[0211] [Evaluation criteria of toluene immersion test]
[0212] A: The ratio of hollow particles precipitated by standing for 120 hours was less than 5% by mass.
[0213] B: The ratio of hollow particles precipitated after being left to stand for 120 hours is 5 mass % or more, and the ratio of hollow particles precipitated after being left to stand for 48 hours is less than 5 mass %.
[0214] X: The ratio of hollow particles precipitated after being left to stand for 48 hours is 5% by mass or more.
[0215] It can be judged that the smaller the ratio of the precipitated hollow particles is, the better the solvent resistance to toluene is.
[0216] <Methyl ethyl ketone immersion test>
[0217] In an environment of 25°C, 0.1 mg of hollow particles were added to 4 mL of methyl ethyl ketone, and the mixture was shaken for 10 minutes at a shaking speed of 100 rpm using an oscillator. After the shaken mixture was left to stand for 24 hours, the hollow particles precipitated in the methyl ethyl ketone were separated by a centrifuge, dried, and the mass of the hollow particles precipitated in the methyl ethyl ketone was measured. Then, the ratio of the mass of the hollow particles precipitated in the methyl ethyl ketone to the mass of the entire hollow particles immersed in the methyl ethyl ketone was calculated to obtain the ratio of the precipitated hollow particles, and the evaluation was performed based on the following evaluation criteria.
[0218] [Evaluation criteria for methyl ethyl ketone immersion test]
[0219] A: The ratio of precipitated hollow particles is less than 5% by mass.
[0220] X: The ratio of precipitated hollow particles is 5% by mass or more.
[0221] <Acetone immersion test>
[0222] 0.1 mg of hollow particles were added to 4 mL of acetone at 25°C, and the mixture was shaken for 10 minutes at a shaking speed of 100 rpm using an oscillator. After the shaken mixture was left to stand for 24 hours, the hollow particles precipitated in the acetone were separated by a centrifuge, dried, and the mass of the hollow particles precipitated in the acetone was measured. Then, the ratio of the mass of the hollow particles precipitated in the acetone to the mass of the entire hollow particles immersed in the acetone was calculated to obtain the ratio of the precipitated hollow particles, and the evaluation was performed based on the following evaluation criteria.
[0223] [Evaluation criteria for acetone immersion test]
[0224] A: The ratio of precipitated hollow particles is less than 5% by mass.
[0225] X: The ratio of precipitated hollow particles is 5% by mass or more.
[0226] <Relative dielectric constant (Dk) and dielectric loss tangent (Df) of hollow particles>
[0227] The hollow particles obtained in each embodiment were measured using a measuring device (AET Co., Ltd., model: ADMS01Nc) to measure the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the hollow particles at a frequency of 1 GHz and room temperature (25°C), and evaluated based on the following evaluation criteria. The lower the relative dielectric constant (Dk), the better the insulation can be judged. In addition, the lower the dielectric loss tangent, the better the insulation can be judged.
[0228] [Evaluation criteria for relative dielectric constant (Dk)]
[0229] A: Relative dielectric constant (Dk) less than 1.55
[0230] B: Relative dielectric constant (Dk) is 1.55 or more and less than 1.57
[0231] C: Relative dielectric constant (Dk) is 1.57 or more and less than 1.60
[0232] X: Relative dielectric constant (Dk) is 1.60 or more
[0233] [Evaluation criteria for dielectric loss tangent (Df)]
[0234] A: Dielectric loss tangent (Df) less than 0.0085
[0235] B: Dielectric loss tangent (Df) is 0.0085 or more and less than 0.010
[0236] C: Dielectric loss tangent (Df) is greater than 0.010 and less than 0.012
[0237] X: Dielectric loss tangent (Df) is 0.012 or more
[0238] [Example 1]
[0239] (1) Mixed solution preparation process
[0240] First, the following materials were mixed to prepare an oil phase.
[0241] Ethylene glycol dimethacrylate 31.85 parts
[0242] 13.65 parts of trimethylolpropane trimethacrylate
[0243] 2,2'-azobis(2,4-dimethylvaleronitrile) 1.04 parts
[0244] Cyclohexane 54.5 parts
[0245] Next, in a stirring tank, an aqueous solution of 16.5 parts of sodium hydroxide (alkali metal hydroxide) dissolved in 55 parts of ion exchange water was slowly added to an aqueous solution of 23.5 parts of magnesium chloride (water-soluble polyvalent metal salt) dissolved in 225 parts of ion exchange water under stirring to prepare a magnesium hydroxide colloid (metal hydroxide colloid hardly soluble in water) dispersion, and stirring was stopped 15 minutes after the addition to prepare an aqueous phase. The obtained aqueous phase was mixed with an oil phase to prepare a mixed solution.
[0246] (2) Suspension process
[0247] Next, the mixed solution obtained in the mixed solution preparation step is used to suspend the mixed solution using a stirring device having an inline emulsifier disperser and a mixed solution supply tank, thereby preparing a suspension in which monomer droplets containing heptane are dispersed in water.
[0248] (3) Polymerization process
[0249] The suspension obtained in the above suspension step was heated to 65°C in a nitrogen atmosphere and stirred at 65°C for 24 hours to perform a polymerization reaction. The polymerization reaction obtained a slurry of precursor particles containing a hydrophobic solvent dispersed in water, that is, a precursor composition.
[0250] (4) Cleaning process and solid-liquid separation process
[0251] The precursor composition obtained in the above polymerization step was washed with dilute sulfuric acid (25°C, 10 minutes) to a pH of 5.5 or less. Then, after separating the water by filtration, 200 parts of ion exchange water was added again for reslurry, and the water washing treatment (washing, filtration, dehydration) was repeated several times at room temperature (25°C), and the solid content was separated by filtration.
[0252] (5) Drying process
[0253] The precursor particles obtained in the solid-liquid separation step were subjected to a 24-hour heat treatment in a vacuum dryer at 200°C to remove water and the encapsulated solvent, thereby obtaining the hollow particles of Example 1. The monomer composition of the shell polymer in the obtained hollow particles is roughly consistent with the composition of the polymerizable monomers used for polymerization. The obtained hollow particles were measured for true density, porosity, volume average particle size (Dv), particle size distribution (Dv / Dn), relative dielectric constant (Dk) and dielectric loss tangent (Df). The results are shown in Table 1.
[0254] [Example 2 to Example 7, Comparative Examples 1 to 4]
[0255] (1) In the mixed solution preparation step, the types and amounts of the monomers, oil-soluble polymerization initiator and hydrophobic organic solvent used in the preparation of the oil phase, the amounts of magnesium chloride and sodium hydroxide used in the preparation of the water phase, and the stirring time during the preparation of the water phase were changed as shown in Table 1, and (3) in the polymerization step, the polymerization temperature was changed as shown in Table 1, and hollow particles were obtained in the same manner as in Example 1. The monomer composition of the shell polymer in the obtained hollow particles was substantially consistent with the composition of the polymerizable monomers used for polymerization. The obtained hollow particles were measured and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0256] In addition, each material used in each Example and each Comparative Example is as follows.
[0257] [monomer]
[0258] EGDMA: Ethylene glycol dimethacrylate (bifunctional heteroatom-containing crosslinking monomer)
[0259] TMPT: Trimethylolpropane trimethacrylate (trifunctional heteroatom-containing crosslinking monomer)
[0260] A-TMMT: Pentaerythritol tetraacrylate (tetrafunctional heteroatom-containing crosslinking monomer)
[0261] St: styrene (monofunctional hydrocarbon monomer)
[0262] Divinylbenzene (bifunctional cross-linking hydrocarbon monomer)
[0263] Ethylvinylbenzene (monofunctional hydrocarbon monomer)
[0264] [Oil-soluble polymerization initiator]
[0265] Initiator 1: 2,2'-azobis(2,4-dimethylvaleronitrile)
[0266] Initiator 2: tert-butyl peroxydiethyl acetate
[0267] [Hydrophobic organic solvent]
[0268] Cyclohexane
[0269] Heptane
[0270] [Table 1]
[0271]
[0272] As shown in Table 1, the hollow particles have a shell composed of a resin and a hollow part surrounded by the shell, and the resin is composed of a shell polymer containing a crosslinkable monomer unit, and the true density is 1.16 g / cm 3 As described above, the hollow particles having a C value of 0.94 or more calculated from the formula (1) have excellent solvent resistance (Examples 1 to 7).
[0273] On the other hand, when the true density of the hollow particles was too small (Comparative Examples 1, 2, and 4) or when the value of C calculated from the formula (1) was too small (Comparative Example 3), the solvent resistance of the hollow particles was poor.
Claims
1. A hollow particle having a shell containing a resin and a hollow portion surrounded by the shell, The resin is composed of a shell polymer containing cross-linkable monomer units, The true density of the hollow particles is 1.16 g / cm 3 above, The value of C of the hollow particles calculated by the following formula (1) is 0.94 or more, C=A×(100-B) / 100 Formula (1) In the above formula (1), A represents the value of the true density of the hollow particles (unit: g / cm 3 ), B represents the content ratio of the monofunctional monomer unit in the shell polymer (unit: mass %).
2. The hollow particles according to claim 1, in, The shell polymer includes a heteroatom-containing monomer unit, and the content ratio of the heteroatom-containing monomer unit in the shell polymer is 80% by mass or more.
3. The hollow particles according to claim 1 or 2, in, The ratio of hollow particles precipitated in the case of immersion in toluene for 48 hours was less than 5% by mass.
4. The hollow particles according to any one of claims 1 to 3, in, The ratio of hollow particles precipitated in the case of immersion in methyl ethyl ketone for 24 hours was less than 5% by mass.
5. The hollow particles according to any one of claims 1 to 4, in, The ratio of hollow particles precipitated in the case of immersion in acetone for 24 hours was less than 5% by mass.
6. The hollow particles according to any one of claims 1 to 5, in, The porosity of the hollow particles is greater than 60%.
7. The hollow particles according to any one of claims 1 to 6, in, The shell polymer includes trifunctional or higher cross-linking monomer units and bifunctional cross-linking monomer units as the cross-linking monomer units.
8. The hollow particles according to claim 7, in, The ratio of the content of the bifunctional crosslinking monomer unit to the content of the trifunctional or higher heteroatom-containing crosslinking monomer unit in the shell polymer is 10:90 to 98:2 in terms of the mass ratio of "bifunctional crosslinking monomer unit:trifunctional or higher heteroatom-containing crosslinking monomer unit".
9. The hollow particles according to any one of claims 1 to 8, in, The volume average particle diameter (Dv) of the hollow particles is 1 to 12 μm.
Citation Information
Patent Citations
Hollow resin particle and method for producing same
WO2021085189A1