Layers comprising calcium carbonate
Through the high load level polyvinyl alcohol and calcium carbonate layers, the problems of limited degradation performance and low calcium carbonate load in the prior art are solved, and the stability and recyclability of high thermal decomposition are achieved, plastic pollution is reduced, and plastics are stabilized in the soil or Adjust pH and promote agricultural growth.
Patent Information
- Application Number
- CN202380028938.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-21
- Filing Date
- 2023-01-20
- Publication Date
- 2024-11-05
Smart Images

Figure BDA0005051369570000081 
Figure BDA0005051369570000091 
Figure BDA0005051369570000121
Abstract
Description
Background Art
[0001] The layer comprising calcium carbonate can be used for various applications. For example, these layers can be used to form containers, paper, paper products, etc. The layer comprises calcium carbonate, polymer (for example polyethylene or other petroleum-based polymers) and optional one or more additional components. However, petroleum-based polymers such as polyethylene have limited degradation properties (for example, insoluble in water) and rely on some compostable conditions and / or additives to accelerate degradation. In addition, this layer comprises the calcium carbonate of relatively low load levels. Summary of the invention
[0002] Embodiments of the present disclosure relate to a layer comprising a relatively high loading level of polyvinyl alcohol and calcium carbonate. For example, embodiments of the layer include polyvinyl alcohol and 20 wt % or more calcium carbonate based on the total weight of the layer. Embodiments of the present disclosure also relate to layers comprising any suitable amount of polyvinyl alcohol and calcium carbonate. DETAILED DESCRIPTION OF THE INVENTION
[0004] In the following detailed description, only some embodiments of the subject matter of the present disclosure are described in an illustrative manner. As will be appreciated by those skilled in the art, the subject matter of the present disclosure can be embodied in many different forms, and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided as examples so that the present disclosure will be thorough and complete, and will fully convey the aspects and features of the present disclosure to those skilled in the art. Therefore, processes, elements and techniques that are unnecessary for a person of ordinary skill in the art to fully understand the aspects and features of the present disclosure may not be described.
[0005] Embodiments of the present disclosure relate to layers comprising polyvinyl alcohol and calcium carbonate (CaCO ). For example, embodiments of the layer include calcium carbonate at a relatively high loading level (e.g., 20 wt % (wt %) or more, 20 wt % or more, or 25 wt % or more, based on the gross weight of the layer). In one or more embodiments, calcium carbonate may be present in an amount of 20 wt % to 97 wt %, 25 wt % to 97 wt %, 35 wt % to 97 wt %, 49 wt % to 97 wt %, 35 wt % to 90 wt %, 49 wt % to 90 wt %, 50 wt % to 97 wt %, 50 wt % to 90 wt %, 51 wt % to 97 wt %, 51 wt % to 90 wt %, 54.5 wt % to 97 wt %, 54.5 wt % to 90 wt %, 55 wt % to 97 wt %, 55 wt % to 90 wt %, 56 wt % to 90 wt %, 57 wt % to 90 wt %, 58 wt % to 90 wt %, 59 wt % to 90 wt %, 60 wt % to 90 wt %, 61 wt % to 90 wt %, 62 wt % to 90 wt %, 63 wt % to 90 wt %, 64 wt % to 90 wt %, 65 wt % to 90 wt %, 66 wt % to 90 wt %, 67 wt % to 90 wt %, 68 wt % to 90 wt % to 97 wt %, 60 wt % to 90 wt %, 61 wt % to 97 wt %, 61 wt % to 97 wt %, 65 wt % to 97 wt %, 65 wt % to 90 wt %, 70 wt % to 97 wt %, 70 wt % to 90 wt %, 71 wt % to 97 wt %, 71 wt % to 90 wt %, 75 wt % to 97 wt %, 75 wt % to 90 wt %, 80 wt % to 97 wt %, 80 wt % to 90 wt %, 81 wt % to 97 wt %, 81 wt % to 90 wt %, or any range of amounts.
[0006] Embodiments of the layer comprising polyvinyl alcohol and calcium carbonate can be used to form mulch films, pesticide containers, coatings, netting, expanded polystyrene box replacements, irrigation drip tapes, fishing nets, fishing lines, cages, plastic bags, net floats, fertilizer containers, plant pots, seedling plugs, plastic tape, ropes, twine, feed bags, twine, greenhouse film, tree guards, pond liners, irrigation pipes, irrigation drippers, ear tags, or harvest crates. The layer comprising polyvinyl alcohol and calcium carbonate can be used in any suitable manner for plants (e.g., crops, fruits, trees, etc.) and / or any suitable activity related to plants, and / or the layer comprising polyvinyl alcohol and calcium carbonate can be used in any suitable manner for animals (e.g., livestock, etc.) and / or any suitable activity related to animals.
[0007] In certain embodiments, the layer comprising polyvinyl alcohol and calcium carbonate can be used in the agricultural industry as a film, sheet or layer to protect and / or warm plants (e.g., by capturing heat from the sun and / or the ambient atmosphere). For example, an embodiment of a layer comprising polyvinyl alcohol and calcium carbonate can be placed over a plant to form an enclosure for the plant (e.g., a polytunnel, polyhouse, hoop house, hoopgreen house, grow tunnel, high tunnel, or greenhouse), and / or the corresponding plant can protrude through a hole (e.g., opening) in the layer comprising polyvinyl alcohol and calcium carbonate, contacting the soil in which the plant is growing, such that the layer comprising polyvinyl alcohol and calcium carbonate warms the soil and prevents or reduces the growth of weeds adjacent to the plant.
[0008] Embodiments utilizing a layer comprising polyvinyl alcohol and calcium carbonate in the agricultural industry reduce the agricultural industry's contribution to plastic pollution and can provide additional benefits. For example, because the layer comprising polyvinyl alcohol and calcium carbonate comprises calcium carbonate, the layer comprising polyvinyl alcohol and calcium carbonate can stabilize or improve the pH of the soil as the layer comprising polyvinyl alcohol and calcium carbonate decomposes and adds calcium carbonate to the soil. In some embodiments, as the layer comprising polyvinyl alcohol and calcium carbonate decomposes, calcium carbonate is added to the soil from the layer comprising polyvinyl alcohol and calcium carbonate, thereby increasing the pH of the soil.
[0009] The layer comprising polyvinyl alcohol and calcium carbonate can be configured to decompose within a set or predetermined time, and the set or predetermined time can be consistent with the pH adjustment time of the soil. For example, the decomposition of the layer comprising polyvinyl alcohol and calcium carbonate and the addition of calcium carbonate to the soil can be configured to correspond to the biological characteristics of the plant being protected and / or warmed by the layer comprising polyvinyl alcohol and calcium carbonate. In some embodiments, the layer comprising polyvinyl alcohol and calcium carbonate can be configured to release calcium carbonate into the soil during a set or predetermined time to control the pH of the soil. In some embodiments, the concentration of calcium carbonate and / or polyvinyl alcohol can be adjusted, and / or a decomposition additive can be included in the layer comprising polyvinyl alcohol and calcium carbonate so that the layer comprising polyvinyl alcohol and calcium carbonate releases calcium carbonate during a set or predetermined time. In some embodiments, the layer comprising polyvinyl alcohol and calcium carbonate can be plowed into the soil so that the layer comprising polyvinyl alcohol and calcium carbonate decomposes and releases calcium carbonate into the soil after plowing into the soil. In some embodiments, based on the degradation rate of the layer comprising polyvinyl alcohol and calcium carbonate, the layer comprising polyvinyl alcohol and calcium carbonate balances the pH of the acidic soil, thereby coordinating the pH of the soil with the pH profile or needs of plants (e.g., crops, fruits, trees, etc.) to maximize or increase agricultural yield and growth performance.
[0010] Embodiments including layers of polyvinyl alcohol and calcium carbonate can form a single material to improve recyclability and / or reuse, for example, when used as silage film. In some embodiments, the layer comprising polyvinyl alcohol and calcium carbonate can include multiple layers that are the same or different from each other. Multiple layers can have degradation rates that are the same or different from each other. In some embodiments, one or more of the multiple layers can include additives (e.g., degradation products), and / or one or more of the multiple layers can be free of or substantially free of additives (e.g., degradation products). As used herein, the term "substantially free of" means that the cited component does not exist, or if present, exists only as incidental impurities.
[0011] The additive may be any suitable additive that accelerates the degradation of polymers commonly used in the art. In some embodiments, the additive may include an oxidatively degradable additive (e.g., an oxidatively biodegradable additive), but the present disclosure is not limited thereto, and the additive may include any suitable additive that accelerates the degradation of polymers commonly used in the art. For example, the additive may not include, and may be completely free of, oxidatively degradable additives and oxidatively biodegradable additives. In some embodiments, the layer comprising polyvinyl alcohol and calcium carbonate is completely free of oxidatively degradable additives and oxidatively biodegradable additives. Based on the gross weight of the layer comprising polyvinyl alcohol and calcium carbonate, the layer comprising polyvinyl alcohol and calcium carbonate may include additives in an amount of 0.01wt% to 20wt% (or 0.01wt% to 10wt%). Additives (e.g., oxidatively degradable additives) may increase the rate at which polymers are oxidatively degraded when exposed to oxygen. For example, oxidatively degradable additives may increase the rate at which polymers are oxidized. When exposed to oxygen, polymers may decompose without the need for bacterial microorganisms to initially decompose the polymer. After the polymer is oxidized (or simultaneously or simultaneously therewith), an organism (e.g., a microorganism, bacteria, and / or the like) may further degrade the remainder of the polymer. This process may be referred to as oxidative biodegradation. Thus, the oxido-degradable additive leads to oxidative biodegradation of the polymer.
[0012] The additive can include any suitable additive that increases polymer oxidation or oxidative-biodegradation rate. The additive can include any non-heavy metal additive or salt that meets EU Packaging Waste Directive 94 / 62 Article 11 and similar U.S. laws and / or regulations. In some embodiments, the oxidatively degradable additive includes salts, such as iron salts, manganese salts, cobalt salts and / or any suitable non-heavy metal salts, but the disclosure is not limited thereto. The term "heavy metal" used herein can refer to those elements restricted in EU Packaging Waste Directive 94 / 62 Article 11. Non-limiting, non-heavy metal, commercially available examples of oxidatively degradable additives include those available from Willow Ridge Plastics Inc. (Erlanger, Kentucky) and / or Bio-Tec Environmental LLC (Cedar Crost, New Mexico).
[0013] In some embodiments, the concentration of the additive can vary from one side of the layer comprising polyvinyl alcohol and calcium carbonate to the other side along a concentration gradient. For example, one side of the layer comprising polyvinyl alcohol and calcium carbonate can be exposed to direct ultraviolet (UV) light (e.g., light from the sun), which catalyzes the decomposition of the layer comprising polyvinyl alcohol and calcium carbonate, resulting in an increase in the degradation rate relative to the side not directly exposed to UV light. Therefore, in some embodiments, the side not directly exposed to UV light can have a relatively high concentration of additives (e.g., degradation products), while the side exposed to UV light can have a relatively low concentration of additives (e.g., degradation products), or can be free of or substantially free of additives, so that the degradation rate of the side directly exposed to UV light is more closely matched to the degradation rate of the side not exposed to UV light. In some embodiments, the concentration of the additive can decrease along a concentration gradient from the side not directly exposed to UV light to the side directly exposed to UV light.
[0014] Any suitable calcium carbonate can be used in the embodiments of the present disclosure. Calcium carbonate can be treated (for example, treated with stearic acid) or untreated. For example, treating calcium carbonate with stearic acid allows the use of higher concentrations of calcium carbonate. Therefore, according to embodiments of the present disclosure, calcium carbonate can be treated with stearic acid to form stearic acid treated calcium carbonate (for example, the reaction product of calcium carbonate and stearic acid) before or during the formation layer. Calcium carbonate can be used together with an additive acting as a lubricant, and the lubricant allows the amount of calcium carbonate to be increased (for example, with an amount greater than 20 wt %, 25 wt % or 35 wt %). Calcium carbonate can be dried before forming a layer. For example, before forming a layer, calcium carbonate can be dried to a moisture content less than 300ppm. Non-restrictive commercially available embodiments of calcium carbonate include Omyacarb OM3 (derived from Omya, Switzerland).
[0015] According to embodiments of the present disclosure, the layer comprises polyvinyl alcohol and calcium carbonate, which can be easily separated by dissolution and / or hydrolysis, thereby allowing the components of the layer to be easily recycled. Without limiting the present disclosure to any particular mechanism, the inventors recognized that calcium carbonate can be easily separated from the layer comprising polyvinyl alcohol and calcium carbonate by dissolution and / or hydrolysis, and that features that were not previously considered for recycling were not considered possible end-of-life scenarios for polyvinyl alcohol and calcium carbonate because polyvinyl alcohol at levels greater than or equal to 5 weight % is not favorable in current recycling.
[0016] If calcium carbonate is combined with polyvinyl alcohol, the calcium carbonate can be recycled, which can provide significant environmental advantages by, for example, reducing the carbon (CO2) footprint of products including polyvinyl alcohol and calcium carbonate. Recovering calcium carbonate from a polymer layer comprising calcium carbonate is novel because calcium carbonate is difficult to separate from existing layers comprising calcium carbonate and polyolefin polymers. Therefore, embodiments of the present disclosure provide a new feature of making the layer recyclable by separating calcium carbonate from polyvinyl alcohol, for example, by dissolution and / or hydrolysis.
[0017] Unlike polymers (except polyethylene terephthalate (PET)), calcium carbonate can be recycled multiple times without (or substantially without) changing the physical properties of the recycled calcium carbonate. By including calcium carbonate at a high loading level, embodiments of the present disclosure provide a layer with excellent strength (e.g., suitable for forming rigid products, such as packaging and / or containers) and comprising a component that can be recycled almost infinitely. For example, the calcium carbonate of this layer can be separated from other components of this layer, and recycled multiple times while calcium carbonate remains recyclable and / or separable. Polyvinyl alcohol can also be recyclable and / or separable, and therefore can also be recycled.
[0018] The separation of calcium carbonate and polyvinyl alcohol can be promoted by the density difference between calcium carbonate and polyvinyl alcohol and / or any other component of this layer. Contrary to the embodiments disclosed by the present invention, polyethylene (or other similar polyolefin polymers) can not be similarly separated from calcium carbonate, thereby making the recycling of the single element (such as polyethylene and calcium carbonate) of the layer comprising polyethylene and calcium carbonate very difficult. For example, the single element of polyethylene and calcium carbonate is just difficult to recycle separately once being combined together. On the contrary, polyvinyl alcohol and calcium carbonate can be separated from the embodiments comprising the layer of polyvinyl alcohol and calcium carbonate, thereby providing the ability of recirculating separately these components from the embodiments disclosed herein.
[0019] In one or more embodiments, calcium carbonate can be separated from the polyvinyl alcohol of the layer by dissolving the polyvinyl alcohol (e.g., by washing with water with or without heating the water) and / or by decomposing the polyvinyl alcohol (e.g., by bacterial digestion of the polyvinyl alcohol). Thus, embodiments of the present disclosure are suitable for use in applications where recycling is beneficial, such as products for fast food and / or fast food restaurants, entertainment venues (e.g., stadiums), vehicles (e.g., aircraft, such as passenger aircraft, and ships, such as cruise ships and naval vessels). For example, according to embodiments of the present disclosure, products including embodiments of the layer can be used on board a ship, and after use, the calcium carbonate can be separated from the polyvinyl alcohol in any suitable manner, the calcium carbonate can be deposited in water (e.g., oceans, lakes, rivers, etc.), and the polyvinyl alcohol (and / or decomposition products and / or other byproducts of the polyvinyl alcohol) can be appropriately disposed of (e.g., can be recycled and / or made into fertilizer).
[0020] Embodiments of the present disclosure also relate to layers comprising any suitable amounts of polyvinyl alcohol (PVOH) and calcium carbonate. Because the melting point of polyvinyl alcohol is relatively higher than, for example, the melting point of polyethylene, embodiments of the layer comprising PVOH and calcium carbonate have relatively high thermal decomposition stability. For example, embodiments of the layer can be thermally stable in air at temperatures up to at least 200°C.
[0021] Unlike polyethylene, polyvinyl alcohol can be hydrolyzed so that polyvinyl alcohol can be dissolved in water. Therefore, an embodiment of a layer including polyvinyl alcohol and calcium carbonate can be immersed in water to dissolve polyvinyl alcohol and separate calcium carbonate from polyvinyl alcohol. Therefore, compared with other products including petroleum-based polymers such as polyethylene, an embodiment of the layer can include hydrolyzable polyvinyl alcohol to increase the rate at which the layer can be degraded or decomposed when the layer is treated. After being dissolved in water, polyvinyl alcohol eventually decomposes into decomposition products (e.g., carbon dioxide, methane, acetate and / or water). Acids and / or alkalis can be used to improve and / or accelerate the hydrolysis and decomposition of polyvinyl alcohol. For example, sodium hydroxide (NaOH) with a low concentration (e.g., pH>9.0) can be used to improve and / or accelerate the hydrolysis and decomposition of polyvinyl alcohol. In some embodiments, if there is protein, NaOH helps protein decomposition. In addition, if there is a metallized layer and / or a plasma layer, the metallized layer and / or the plasma layer will be separated from the other components of the layer.
[0022] Compared with uncrosslinked polyvinyl alcohol, crosslinked polyvinyl alcohol can reduce the rate of polyvinyl alcohol hydrolysis. For example, an embodiment of uncrosslinked polyvinyl alcohol can be dissolved in water at a temperature of 12°C, and an embodiment of crosslinked polyvinyl alcohol is thermally stable in water at a temperature of up to 40°C or 90°C. By having high thermal stability (e.g., thermal stability at a temperature of up to 30°C or 150°C), the function of polyvinyl alcohol can be improved and its use can be expanded. Crosslinked polyvinyl alcohol can increase the rigidity of the resulting layer comprising crosslinked polyvinyl alcohol. In addition to increasing the rigidity of the resulting layer, crosslinking polyvinyl alcohol can increase the amount of calcium carbonate that can be included in the resulting layer comprising crosslinked polyvinyl alcohol. The crosslinking of polyvinyl alcohol will also increase the adhesion between calcium carbonate and polyvinyl alcohol, which leads to higher tensile strength. Polyvinyl alcohol can be crosslinked in any suitable manner and is not limited to any particular method or crosslinking agent. For example, polyvinyl alcohol can be crosslinked by chemical crosslinking by inserting acid groups, bases (e.g., basic groups) and / or mixtures or combinations thereof. Due to the hydrophilic nature of polyvinyl alcohol, the free hydroxyl groups of polyvinyl alcohol can be crosslinked to the functional groups of the crosslinking agent. The following cross-linking agents are non-limiting examples of cross-linking with polyvinyl alcohol and improving the thermal stability of polyvinyl alcohol: sulfonic acid groups and carboxylic acid groups, such as sulfosuccinic acid and citric acid. In addition, non-limiting examples of cross-linking agents include glutaraldehyde, formaldehyde, ferrous sulfate heptahydrate, hydrogen peroxide and sodium hydroxide. For example, polyvinyl alcohol can be cross-linked using citric acid and / or aldehyde as a cross-linking agent. In one or more embodiments, cross-linking can include oxygen atoms. Including cross-linked polyvinyl alcohol in the layer can also increase the strength and / or rigidity of the layer. Therefore, the embodiment of the layer can include cross-linked polyvinyl alcohol to increase the water resistance of the layer, increase the strength of the layer and / or increase the rigidity of the layer.
[0023] The composition of polyvinyl alcohol is not particularly limited, and any suitable polyvinyl alcohol available in the art can be used. The embodiment of polyvinyl alcohol may have a high hydroxyl content and high hygroscopicity. The hydroxyl content of polyvinyl alcohol may be any suitable amount commonly used in the art. In some embodiments, the hydroxyl content is 24 to 47 mol%. The hydroxyl content of polyvinyl alcohol reflects the number of hydroxyl groups present in polyvinyl alcohol. The % of hydroxyl corresponds to the number of hydroxyl groups present in polyvinyl alcohol, and therefore, the higher the % of hydroxyl, the higher the number of hydroxyl groups in polyvinyl alcohol. As the hydroxyl content of polyvinyl alcohol increases, polyvinyl alcohol is more susceptible to hydrolysis and becomes more miscible with water. In addition, increasing the hydroxyl content of polyvinyl alcohol increases the number of potential cross-linking sites of polyvinyl alcohol. Non-limiting commercially available embodiments of polyvinyl alcohol include Auqapak Hydropol30164P (available from Aquapak Polymers Ltd., Birmingham, United Kingdom) and any suitable polyvinyl alcohol available from Kuraray (Chiyoda City, Tokyo, Japan), such as POVALTM.
[0024] The inclusion of polyvinyl alcohol in the layer also allows the amount of calcium carbonate in the layer to be significantly increased compared to a layer comprising polyethylene. For example, for a layer comprising polyethylene, the viscosity of the composition used to form the layer increases with increasing amount of calcium carbonate, resulting in a corresponding increase in processing difficulty using existing equipment. For a layer comprising polyethylene, the processing temperature of the composition used to form the layer increases with increasing amount of calcium carbonate in order to reduce the viscosity of the composition to a level suitable for processing, thereby increasing the energy intensity of the method.
[0025] For a layer comprising polyvinyl alcohol, even when the amount of calcium carbonate is increased to a high level (e.g., 20% to 97%, 25% to 97% or 35% to 97% by weight, based on the total weight of the layer), the viscosity of the composition used to form the layer can be reduced by adding water and / or by adding a viscosity reducer (e.g., glycerol, low molecular weight PHA (polyhydroxyalkanoate), PLA (polylactic acid) and / or polyethylene glycol), thereby improving the processability of the composition. Therefore, embodiments of a layer comprising polyvinyl alcohol and calcium carbonate can be processed even at high loading levels of calcium carbonate (e.g., 20% to 97%, 25% to 97% or 35% to 97% by weight, based on the total weight of the layer). According to embodiments of the present disclosure, water can be added to the composition for forming a layer comprising polyvinyl alcohol and calcium carbonate to reduce the viscosity of the composition, and then at least a portion of the water can be subsequently removed, and / or additives such as starch, gluten, cellulose and / or industrial proteins can be added to increase the viscosity after and / or during processing. Embodiments comprising layers of polyvinyl alcohol and calcium carbonate can be processed and / or formed using existing mixing and extrusion equipment for processing polyethylene resins. In one or more embodiments, the polyvinyl alcohol can be handled, stored and / or processed in any suitable manner to avoid or reduce moisture absorption, such as handling, storing and / or processing with a suitable desiccant and / or under a nitrogen atmosphere.
[0026] Embodiments of layers including polyvinyl alcohol and calcium carbonate may exhibit a synergistic effect due to the combination of polyvinyl alcohol and calcium carbonate. For example, while a layer comprising relatively pure polyvinyl alcohol may exhibit a significant decrease in strength after 5 months, a layer comprising polyvinyl alcohol and 50 wt % calcium carbonate based on the total weight of the layer exhibits substantially the same strength (e.g., tensile strength in MPa or psi) after 5 months. Stress / strain data for examples and comparative examples of embodiments of the present disclosure are shown below.
[0027]
[0028]
[0029] *Sec.Mod.=Secant modulus
[0030] *psi = pounds per square inch
[0031] *MPa = Megapascal
[0032] As can be seen above, all conditions of the examples were harder when CaCO3 was added.
[0033] As described in the following examples, after 8 weeks under ambient conditions, the stiffness of the untreated strip comprising polyvinyl alcohol and 40% CaCO3 was 57% of the initial stiffness, while after 8 weeks under ambient conditions, the stiffness of the treated strip comprising polyvinyl alcohol and 40% CaCO3 was 81% of the initial stiffness. Therefore, the embodiment of the layer comprising polyvinyl alcohol and calcium carbonate shows unexpected and beneficial property changes. Although the present disclosure is not limited by any particular mechanism or theory, it is believed that the chemical bond and / or physical interaction between polyvinyl alcohol and calcium carbonate provide unexpected and beneficial increases in strength and / or stiffness. These unexpected beneficial effects can increase with the increase of the amount of calcium carbonate (for example, increase to 70% by weight or more based on the gross weight of the layer). For example, although not limited by any particular mechanism or theory, it is believed that the calcium carbonate particles surrounded by a relatively small amount of polyvinyl alcohol at least in part provide excellent strength and rigidity. According to an embodiment of the present disclosure, calcium carbonate provides compression resistance for the layer, while the layer maintains the strain resistance of polyvinyl alcohol.
[0034] The layers of the present disclosure are not limited to monolayers. For example, embodiments of the present disclosure may also include multiple layers including multiple layers comprising calcium carbonate and / or multiple layers comprising polyvinyl alcohol and calcium carbonate. Multiple layers may be physically or directly in contact with one or more of each other, or may have additional elements or features therebetween.
[0035] In one or more embodiments, multilayer comprises a layer containing polyvinyl alcohol and calcium carbonate, and a protective layer on one or more sides of the layer containing polyvinyl alcohol and calcium carbonate. In one or more embodiments, the layer comprising polyvinyl alcohol and calcium carbonate can be used as a layer or coating on paper or paperboard. The layer comprising polyvinyl alcohol and calcium carbonate on paper or paperboard provides greater rigidity for paper or paperboard than the layer containing only polyvinyl alcohol. Multilayer may include any suitable layer used in the art, and may include a layer containing polyethylene in some embodiments. For example, multilayer may include a layer containing polyvinyl alcohol and calcium carbonate, or a layer containing polyvinyl alcohol and calcium carbonate, and on a first side of a layer containing polyvinyl alcohol and calcium carbonate or a layer containing polyvinyl alcohol and calcium carbonate, on a second side of a layer containing polyvinyl alcohol and calcium carbonate or a layer containing polyvinyl alcohol and calcium carbonate, or a protective layer on both. In the embodiment of a container or straw comprising a layer containing polyvinyl alcohol and calcium carbonate, the first side may be the inner side, and the second side may be the outer side. The protective layer can protect the layer comprising polyvinyl alcohol and calcium carbonate from oxidants (e.g., oxygen), moisture (e.g., water or water vapor), and / or acids, and / or the protective layer can prevent the contents of the container comprising the layer of polyvinyl alcohol and calcium carbonate from physical contact with the polymer (e.g., polyvinyl alcohol) of the layer. The protective layer can include any suitable material. For example, the protective layer can include a metallized film, e.g., an aluminized film, and / or the protective layer can include a plasma layer.
[0036] In some embodiments, a condensed plasma layer having a thickness of 5 to 500 nanometers is applied to a PVOH / CaCO3 film to produce a novel packaging material. The condensed plasma layer has several functions, including, for example, as a barrier layer for degradation of the PVOH / CaCO3 composite and as a sacrificial layer that can be removed under specific conditions to initiate composite degradation. In this embodiment, the condensed plasma coating is an aluminum oxide or silicon dioxide layer that can be etched or degraded by a strong base such as NaOH. In another embodiment, the condensed plasma coating is used to meet currently existing government regulations that prohibit the use of polymer packaging to contact tobacco or related types of materials. Therefore, embodiments of the present disclosure including condensed plasma coatings are expected to have similar or better properties of less environmentally harmful packaging.
[0037] The deposition of the condensed plasma layer on the film can be carried out by physical vapor deposition using an electron beam emitter to heat aluminum oxide or silicon dioxide and produce a vapor plasma cloud of molecules. The process can be carried out in a closed area under vacuum or atmospheric conditions, wherein the film passes through the closed area. The plasma molecules move to the surface of the film and condense into a uniform (e.g., substantially uniform) very thin layer of about 5 to 500 nanometers. The thin layer of the condensed plasma layer is sufficient to impart certain properties to the substrate / film, including a barrier to oxygen, moisture, and / or certain UV radiation.
[0038] In one or more embodiments, the aluminized film may be thinner than the aluminized film used in the existing layer. For example, the aluminized film of one or more embodiments of the present application may include 0.125wt% of aluminum used in the existing aluminized film. In one or more embodiments, the protective layer includes an oxide, such as a metal oxide (e.g., aluminum oxide, Al2O3). When the embodiment of the layer including the protective layer is dissolved, the calcium carbonate and the components of the protective layer (e.g., metal) can be separated from the polyvinyl alcohol, and therefore, the metal can also be recyclable and / or recyclable.
[0039] The layer according to the embodiment of the present disclosure may also include any suitable additive or other component. For example, the embodiment of the layer may include additives, such as cellulose and / or protein (e.g., industrial protein), to increase the strength and / or rigidity of the layer. Due to their viscoelasticity, proteins can have the ability to increase the toughness and tensile strength of polyvinyl alcohol, or can be used alone. When proteins are included in the layer, care should be taken to ensure that the processing temperature of the layer does not exceed the denaturation temperature of the protein. In some embodiments, the layer may include 25 to 30% by weight of protein, 0.1 to 5% by weight of polyvinyl alcohol, and 70 to 90% by weight of calcium carbonate.
[0040] Embodiments of the present disclosure can be used to form a variety of products, such as transparencies (e.g., for vehicles and / or electronic devices), containers, wrappers, straws, films, cups, plates, product bags (e.g., tobacco pouches), tableware, rigid packaging, etc., but the present disclosure is not limited thereto. The container may have a main body that limits the inner cavity that can hold articles (e.g., solids, liquids, and / or gases). The main body of the container may include a layer containing polyvinyl alcohol and calcium carbonate or may be formed by a layer containing polyvinyl alcohol and calcium carbonate. Any product disclosed herein may be flexible or rigid, or may have a flexible part and / or a rigid part. In some embodiments, the packaging material may be a food packaging material, such as a sandwich packaging material (e.g., a hamburger and / or cheeseburger packaging material), a hot dog packaging material, etc. In some embodiments, the container may include a sealed bag (e.g., a bag that contains or will contain potato chips, popcorn, and / or the like), an unsealed bag (e.g., a grocery bag), a package (e.g., a package that contains or will contain snack bars, health bars, and / or the like), a blister package (e.g., a blister package that contains or will contain medications and / or the like), a bag, a candy package (e.g., a package that contains or will contain candy, ice cream, and / or the like), a cereal bag (e.g., a bag that contains or will contain cereal products and / or the like), a dairy container, a bottle (e.g., a bottle containing a carbonated beverage, such as, for example, a bottle of beer and / or the like), a box (e.g., a box that contains or will contain beer, wine, juice, soup, and / or the like), a can, a bread bag (e.g., a bag that contains or will contain bread), a bagel bag (e.g., a bag that contains or will contain bagels), a container that contains or will contain produce, an air bag, and / or the like, but the present disclosure is not limited thereto. In some embodiments, a layer comprising polyvinyl alcohol and calcium carbonate can be used to form a tobacco pouch, wherein the tobacco is not in physical contact with the polyvinyl alcohol of the layer due to the presence of the protective layer.
[0041] According to embodiments of the present disclosure, the layer comprising polyvinyl alcohol and calcium carbonate can be formed according to any suitable method. For example, embodiments of the present disclosure can be formed using a high sprue or pocket bubble blown film extrusion process for making microporous, paper-like films. Rigid embodiments of the layer can be formed by any suitable process, such as thermoforming, injection molding, profile extrusion, blow molding, etc. For example, the layer comprising polyvinyl alcohol and calcium carbonate can be molded to, for example, form a pesticide bottle, irrigation pipe, etc., or the layer comprising polyvinyl alcohol and calcium carbonate can be thermoformed to, for example, form a seedling tray, seedling tray, etc.
[0042] Embodiments of the present disclosure will now be described in more detail with reference to prophetic examples. The prophetic examples are provided only to illustrate embodiments of the present disclosure, and the present disclosure is not limited thereto.
[0043] Prophetic examples of layers that can be formed include calcium carbonate in amounts of 51 wt%, 54.5 wt% and 65 wt% based on the total weight of each layer, respectively. According to the prophetic examples, a portion of the polyvinyl alcohol can be replaced with starch (e.g., thermoplastic potato starch (TPS), such as Bioplast 300, available from BIOTEC GmbH, Rhein, Germany). The polyvinyl alcohol may be cross-linked according to any suitable method, such as heat cross-linking, microwave cross-linking, ultrasonic cross-linking, citric acid cross-linking (e.g., cross-linking using citric acid as a cross-linking agent, sodium borate cross-linking (e.g., cross-linking using sodium borate (borax) as a cross-linking agent), etc. Therefore, according to embodiments of the present disclosure, cross-linking changes the physical properties of the resulting layer without (or substantially) reducing the biodegradability of the layer (e.g., the cross-linking may be sufficiently low that it does not (or substantially) interfere with the biodegradability of the resulting layer). Although subjecting the polyvinyl alcohol to a high temperature cross-linking process may denature the polyvinyl alcohol, the denatured components may recombine in the presence of calcium carbonate, thereby making the resulting package more resistant to hydrolytic decomposition. According to a prophetic embodiment, citric acid may be added as a cross-linking agent to stabilize the polyvinyl alcohol and provide enhanced mechanical properties and adhesion to calcium carbonate. The composite strands of the prophetic embodiment may be cold air dried, pelletized, and stored in foil bags to avoid or reduce moisture absorption.
[0044] According to a prophetic embodiment, the compound and the polyvinyl alcohol source can be extruded using a Haake horizontal sheet extruder and a cooling roll traction system. Any suitable cooling method, such as air cooling, belt conveyor cooling and / or the like. The product can be produced in the form of a strip having a thickness and width equal to the size of existing polypropylene straws. The compounding conditions of the prophetic embodiment are shown in Table 1 below.
[0045] Table 1
[0046]
[0047]
[0048] The compounder starting temperature settings and rates for Prophetic Examples 1-5 are shown in Table 2 below.
[0049] Table 2
[0050]
[0051] Haake sheet extrusion process parameters
[0052] All mixing conditions and polyvinyl alcohols (one or both of the polyvinyl alcohols shown in Table 1) were extruded into 0.75 inch (19.05 mm) thick tapes of 8.00-8.50 mils (0.203-0.216 mm) according to the parameters shown in Table 3 below.
[0053] Table 3
[0054] Extrusion temperature -220℃ / -220℃ / 200℃ / 200℃ Expected melting temperature -195℃ Cooler temperature 20℃ Pull distance from mold 9 inches (22.86 cm) at maximum speed
[0055] Storage of materials and samples
[0056] Samples of the polymer source, composite pellets, and tape will be collected and packaged in foil moisture barrier bags for analysis. The composites are collected and stored in foil moisture bags until ready for extrusion. In one or more embodiments, drying can be performed prior to compounding.
[0057] stability
[0058] The tapes prepared according to the above Haake sheet extrusion process were stored at ambient conditions for 8 weights. The tapes were produced by feeding the compound into the feed throat of the extruder, where the material was melted and plasticized under pressure, and exited from the horizontal die to a 3-roll stack cooler system to form an S-shaped package. The film was stretched to the desired width and thickness and optimized by the speed of the rollers.
[0059] Strip preparation
[0060] The Haake is preheated and allowed to soak for 1 hour. The pellets are loaded into the Haake hopper. After the hopper is loaded, the screw begins to rotate to the set speed (rpm). The compound becomes molten as it moves downstream to the die exit. The molten material leaves the horizontal die and forms a strip under pressure. The strip is then directed to a cooling roller to form an "S" shaped package. The cooled material unwinds from the cooling roller and is pulled down onto the rollers. The roller speed is adjusted to pull the strip down to the desired thickness and width.
[0061] After 8 weeks, a significant difference in hardness was observed for the untreated strips containing 40% CaCO3 relative to the treated strips containing 40% CaCO3.
[0062] Test Method
[0063] Secant modulus 1% (strip stiffness) was measured according to ASTM D-882 method: crosshead speed 0.200 inches / minute, 500N load cell. Strip thickness and width were measured and entered into the program. After the strip was mounted between two clamps with a 5-inch gauge length, the crosshead speed was started and a stress / strain curve was generated. The secant modulus 1% value was calculated and recorded. After 8 weeks at ambient conditions, the stiffness of the untreated strip containing 40% CaCO3 was 57% of the initial stiffness, while after 8 weeks at ambient conditions, the stiffness of the treated strip containing 40% CaCO3 was 81% of the initial stiffness. After 8 weeks at ambient conditions, the treated strip containing 55% CaCO3 showed no loss of hardness. The purpose of preparing the above-mentioned strips is to produce strips (e.g., 1.0 inch width and 8.5 mil thickness) that simulate open commercial straws. As the CaCO3 level (or amount) increases, the method stabilizes and the strips become more consistent, allowing the widest strip width at 55% CaCO3.
[0064] Table 4
[0065]
[0066]
[0067] As used herein, the term "layer" can be used interchangeably with the term "film", and these terms can be given the same or substantially the same meaning. In addition, it will be understood that although the terms "first", "second", "third", etc. can be used to describe various elements, components, regions, layers and / or parts in this article, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are used to distinguish an element, part, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the spirit and scope of the present disclosure, the first element, component, region, layer or part described below can be referred to as the second element, component, region, layer or part.
[0068] For ease of explanation, spatially relative terms such as "below", "lower", "below", "above", "upper" and the like may be used herein to describe the relationship of one element or feature to another element or feature. It should be understood that, in addition to the described orientations, spatially relative terms are also intended to include different orientations of the device in use or operation. For example, if the device is flipped, an element described as being "below" or "under" or "below" other elements or features will be oriented as being "above" other elements or features. Therefore, the exemplary terms "below" and "below" may include orientations of above and below. The device may be oriented in other ways (e.g., rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein should be interpreted accordingly.
[0069] It will be understood that when an element or layer is referred to as being "on," "connected to," or "coupled to" another element or layer, it can be directly on, directly connected to, or directly coupled to the other element or layer, or one or more intervening elements or layers may be present. Additionally, it will be understood that when an element or layer is referred to as being "between" two elements or layers, it can be the only element or layer between the two elements or layers, or one or more intervening elements or layers may also be present.
[0070] The terms used herein are only used to describe the purpose of a particular embodiment, and do not wish to limit the present invention. As used herein, the singular "one" and "an" are also intended to include plural forms, unless the context clearly indicates otherwise. It will also be understood that the terms "include" and "comprise" specify the existence of stated features, integers, actions, operations, elements and / or components when used in this specification, but do not exclude the existence or addition of one or more other features, integers, actions, operations, elements, components and / or their combinations. As used herein, the term "and / or" includes any and all combinations of one or more associated listed items. When before an element list, expressions such as "at least one" modify the entire element list without modifying the individual elements of the list.
[0071] As used herein, the terms "substantially," "approximately," and similar terms are used as terms of approximation rather than terms of degree, and are intended to account for the inherent deviations in measurements or calculations that one of ordinary skill in the art would recognize. Additionally, the use of "may" when describing embodiments of the present disclosure refers to "one or more embodiments of the present disclosure." As used herein, the terms "use," "using," and "used" may be considered synonymous with the terms "utilizing," "utilizing," and "utilized," respectively. Additionally, the term "exemplary" is intended to refer to an example or illustration.
[0072] In addition, any numerical range cited herein is intended to include all subranges of the same numerical precision contained within the cited range. For example, the range of "1.0 to 10.0" is intended to include all subranges between (and including) the minimum value 1.0 and the maximum value 10.0, that is, having a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as 2.4 to 7.6. Any maximum numerical limit described herein is intended to include all lower numerical limits contained therein, and any minimum numerical limit described in this specification is intended to include all higher numerical limits contained therein. Therefore, the applicant reserves the right to modify this specification, including the claims, to explicitly list any subranges contained within the range explicitly listed herein.
[0073] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It should also be understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology and / or this specification, and should not be interpreted in an idealized or overly formal sense, unless explicitly defined as such herein.
[0074] While the disclosed subject matter has been described in conjunction with certain embodiments, it should be understood that the disclosed subject matter is not limited to the disclosed embodiments, but on the contrary, the disclosure is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims and their equivalents.
Claims
1. A layer comprising: Polyvinyl alcohol; as well as 20 wt% or more calcium carbonate, based on the total weight of the layer.
2. The layer according to claim 1, wherein the calcium carbonate comprises stearic acid treated or untreated calcium carbonate.
3. The layer of claim 1, wherein the polyvinyl alcohol is cross-linked.
4. The layer according to claim 1, wherein the layer comprises calcium carbonate in an amount of 50 wt.-% to 97 wt.-%, based on the total weight of the layer.
5. The layer according to claim 1, wherein the layer comprises calcium carbonate in an amount of 70 to 97 wt.-%, based on the total weight of the layer.
6. The layer according to claim 1, further comprising a protective layer on one side of the layer, which protects the layer comprising polyvinyl alcohol and calcium carbonate from oxidants, moisture and / or acids, and / or can protect the layer comprising polyvinyl alcohol and calcium carbonate from physical contact with the contents of a container of the layer comprising polyvinyl alcohol and calcium carbonate.
7. The layer of claim 6, wherein the protective layer comprises a plasma coating.
8. The layer of claim 1, wherein the layer is thermally stable at temperatures up to 150°C.
9. The layer of claim 1, wherein the layer further comprises a protein.
10. A container comprising: a body defining an interior cavity capable of holding an item, wherein the body comprises a layer, the layer comprising: Polyvinyl alcohol; and 20 wt% or more calcium carbonate, based on the total weight of the layer.
11. The container of claim 10, wherein the calcium carbonate comprises stearic acid treated calcium carbonate.
12. The container of claim 11, wherein the polyvinyl alcohol is cross-linked.
13. The container of claim 10, wherein the layer comprises calcium carbonate in an amount of 50 wt% to 97 wt% based on the total weight of the layer.
14. The container of claim 10, wherein the layer comprises calcium carbonate in an amount of 70 wt% to 97 wt% based on the total weight of the layer.
15. The container according to claim 10, further comprising a protective layer on one side of the layer, the protective layer protecting the layer comprising polyvinyl alcohol and calcium carbonate from oxidants, moisture and / or acids, and / or can protect the layer comprising polyvinyl alcohol and calcium carbonate from physical contact with the contents of the container.
16. The container of claim 15, wherein the protective layer comprises a plasma coating.
17. The container of claim 10, wherein the layer is thermally stable at temperatures up to 150°C.
18. The container of claim 10, wherein the layer further comprises a protein.
19. A container comprising: Layer, which contains: Polyvinyl alcohol; and Calcium carbonate.
20. The container of claim 19, wherein the layer comprises calcium carbonate in an amount of 50 wt% to 97 wt%, based on the total weight of the layer.
21. The container according to claim 19, further comprising a protective layer on one side of the layer, the protective layer protecting the layer comprising polyvinyl alcohol and calcium carbonate from oxidants, moisture and / or acids, and / or can protect the layer comprising polyvinyl alcohol and calcium carbonate from physical contact with the contents of the container comprising the layer comprising polyvinyl alcohol and calcium carbonate.
22. The container of claim 21, wherein the protective layer comprises a plasma coating.
23. The container of claim 21, wherein the layer is thermally stable at temperatures up to 150°C.
24. The container of claim 21, wherein the layer further comprises a protein.