Method and apparatus for producing waste plastic pyrolysis oil with reduced chlorine content
Through the X-ray diffraction analysis and pyrolysis process of modified red mud, the chlorine content in the pyrolysis oil of waste plastics is reduced, and the problems of high chlorine content in the pyrolysis oil of waste plastics are solved and the difficulty in handling red mud is achieved, achieving high quality Production of pyrolytic oil and efficient utilization of resources.
Patent Information
- Application Number
- CN202380032517.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-04
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The high chlorine content in the pyrolytic oil of waste plastics leads to equipment corrosion and product performance deterioration during the hydrotreatment process. The treatment of red mud has huge facilities costs and environmental pollution problems, which are difficult to directly utilize.
Modified red mud for X-ray diffraction analysis, with a specific peak intensity ratio of more than 5 to reduce the chlorine content in the pyrolysis oil of waste plastics, and perform a pyrolysis process in a non-oxidizing atmosphere of 300-600℃, using modification The excellent chlorine adsorption properties of pyrogenic red mud reduce chlorine content.
It effectively reduces the chlorine content in waste plastic pyrolytic oil, reduces the demand for post-treatment process, improves the quality and production efficiency of pyrolytic oil, reduces process costs, and solves the environmental and economic problems of red mud treatment.
Smart Images

Figure CN118900907A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing pyrolysis oil with reduced chlorine content from waste plastics. Background Art
[0002] Waste plastics are difficult to recycle and are mostly disposed of as garbage. These wastes take a long time to degrade in nature, causing soil contamination and serious environmental pollution. As a method of recycling waste plastics, a method of converting waste plastics into oil through a pyrolysis process was conducted.
[0003] However, the pyrolysis oil obtained by pyrolyzing waste plastics cannot be directly used as a high-value-added fuel such as gasoline or diesel because the pyrolysis oil has a higher content of impurities such as chlorine, nitrogen, metals and solid by-products compared to fractions produced from crude oil by conventional methods. Therefore, the pyrolysis oil can be used as a fuel after adsorbing impurities through a refining process.
[0004] For example, by hydrotreating waste plastic pyrolysis oil in the presence of a hydrotreating catalyst, chlorine is converted into hydrogen chloride and adsorbed. However, the chlorine content in waste plastic pyrolysis oil is high, so excessive hydrogen chloride is produced during the hydrotreating process, leading to problems such as equipment corrosion, abnormal reactions, and deterioration of product performance.
[0005] In addition, a technique using an adsorbent such as CaO or an effluent catalytic cracking (FCC) catalyst (E-cat) has been used to adsorb chlorine, nitrogen, etc. However, in order to achieve the adsorption effect, the amount of the adsorbent used should be quite high (2-50 times the content of the oil to be refined), and the deactivated adsorbent should be constantly replaced because the adsorption effect is lost after adsorbing chlorine, nitrogen, etc.
[0006] Therefore, there is a need for a method for producing waste plastic pyrolysis oil with a reduced chlorine content to a level that can be introduced into a refining process.
[0007] Meanwhile, red mud is a waste product produced during the extraction of alumina from bauxite. More than 120 million tons of red mud in the form of sludge and more than 40 million tons of red mud in the form of dry powder are discharged worldwide each year, and the amount is increasing. In South Korea, more than 200,000 tons of red mud are discharged in the form of sludge each year.
[0008] As the treatment method of red mud, the method utilizing red mud in building materials, the method utilizing red mud as heavy metal treatment agent, etc. have been adopted. However, because red mud has strong alkalinity and high water content, there are many restrictions in utilizing red mud. At present, the utilization of red mud must go through pre-treatment process, which has caused serious problems such as huge facility cost and processing cost required for drying and grinding red mud, and environmental damage caused by dust. Because red mud cannot be landfilled, there is no suitable place to load red mud, and the leakage of leachate (leachate) can cause damage to nearby crops and human life. Therefore, processing red mud is extremely urgent. Summary of the invention
[0009] Technical issues
[0010] An object of the present invention is to provide a method for producing pyrolysis oil of waste plastics, which method can utilize red mud, a waste, as a useful resource and can effectively reduce the chlorine content in the pyrolysis oil produced by pyrolysis of waste plastics.
[0011] Another object of the present invention is to provide a technology for minimizing the chlorine content in pyrolysis oil produced by using modified red mud having a maximum chlorine adsorption effect.
[0012] Another object of the present invention is to provide a pyrolysis oil having a low impurity content level suitable for refining process without the need for additional post-treatment process after pyrolysis of waste plastic feedstock.
[0013] Technical solutions to technical problems
[0014] In a general aspect, a method for producing waste plastic pyrolysis oil with reduced chlorine content includes: a first step of charging a waste plastic raw material and modified red mud into a reactor; and a second step of pyrolyzing the waste plastic raw material in the reactor and recovering the pyrolysis oil, wherein, when the modified red mud is subjected to X-ray diffraction (XRD) analysis, the intensity of a first peak with a 2θ diffraction angle of 14±0.1° is higher than the intensity of a second peak with a 2θ diffraction angle of 14.5±0.1°.
[0015] In one embodiment, the ratio (I1) / (I2) of the intensity of the first peak (I1) to the intensity of the second peak (I2) may be 5 or more.
[0016] In one embodiment, the ratio (I1) / (I3) of the intensity of the first peak (I1) to the intensity of the third peak (I3) may be 5 or more.
[0017] In one embodiment, in the first step, the modified red mud may be charged into the reactor in an amount of 5-30 parts by weight relative to 100 parts by weight of the waste plastic raw material.
[0018] In one embodiment, in the first step, the modified red mud may be charged into the reactor in a paste form by further containing moisture, and the amount of the moisture is 30-80 parts by weight relative to 100 parts by weight of the modified red mud.
[0019] In one embodiment, the second step may be performed at a temperature of 300-600°C.
[0020] In one embodiment, the second step may be performed in a non-oxidizing atmosphere.
[0021] Beneficial Effects
[0022] As described above, in the method for producing waste plastic pyrolysis oil, the chlorine content in the pyrolysis oil can be effectively reduced by pyrolyzing the waste plastic in the presence of modified red mud.
[0023] According to the method for producing waste plastic pyrolysis oil of the present invention, pyrolysis oil with a low impurity content level suitable for a refining process can be produced without additional post-processing after pyrolysis of the waste plastic raw materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Graphs showing the results of X-ray diffraction (XRD) analysis of red mud of Example 3 and Comparative Example 1 as representative examples of the present invention. DETAILED DESCRIPTION
[0025] Unless the context clearly indicates otherwise, the singular forms of the terms used in this specification may be construed as including the plural forms.
[0026] The numerical range used in this specification includes upper and lower limits and all values within these limits, all double limits, and all possible combinations of upper and lower limits within the numerical range defined in different forms. Unless otherwise clearly defined in this specification, values that may exceed the numerical range due to experimental errors or rounding also belong to the defined numerical range.
[0027] The expression "comprising" in this specification is intended to be an open transition phrase, which means equivalent to "including", "containing", "having" or "characterized by", and does not exclude all elements, materials or steps not further described in this document.
[0028] Unless otherwise defined, the unit "%" used in the present specification means "% by weight".
[0029] Unless otherwise defined, the unit "ppm" used in this specification means "mass ppm".
[0030] Waste plastics include polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polystyrene (PS), etc., and waste plastics contain organic chlorine and inorganic chlorine. The pyrolysis oil produced by the pyrolysis process of waste plastics cannot be directly used as a high value-added fuel such as gasoline or diesel due to its high impurity content. Therefore, the pyrolysis oil can be used as a fuel after adsorbing impurities through a refining process. Therefore, a technology for producing pyrolysis oil of waste plastics with minimized chlorine content is needed.
[0031] Meanwhile, red mud is a waste product generated in the process of extracting alumina from bauxite, and ordinary red mud is discharged in the form of sludge with a water content of about 30% to 50%. Ordinary red mud in a high water content state is usually dried through a pretreatment process and then used as a building material, heavy metal treatment agent, etc. Such a pretreatment process requires huge facility costs and processing costs, especially the drying process will change the physical and chemical properties of the red mud, so there are many limitations in the use of red mud.
[0032] Therefore, the present invention provides a method for effectively reducing chlorine in pyrolysis oil produced in a waste plastic pyrolysis process using modified red mud having maximum selectivity and adsorption characteristics for chlorine.
[0033] Specifically, one embodiment of the present invention provides a method for producing pyrolysis oil of waste plastics with reduced chlorine content, the method comprising: a first step of charging a waste plastic raw material and modified red mud into a reactor; and a second step of pyrolyzing the waste plastic raw material in the reactor and recovering the pyrolysis oil, wherein when the modified red mud is subjected to X-ray diffraction (XRD) analysis, the intensity of a first peak with a 2θ diffraction angle of 14±0.1° is higher than the intensity of a second peak with a 2θ diffraction angle of 14.5±0.1°. X-ray diffraction (XRD) analysis refers to an X-ray diffraction pattern using CuKα rays.
[0034] Specifically, when performing X-ray diffraction (XRD) analysis, the intensity of the first peak at a 2θ diffraction angle of 14±0.1° is higher than the intensity of the second peak at a 2θ diffraction angle of 14.5±0.1°, and the modified red mud has significantly excellent selectivity for chlorine and chlorine adsorption characteristics in the pyrolysis process. In the case of using the red mud of the related art, the red mud is dried at 110°C for 24 hours and used in the form of dry red mud. On the other hand, the modified red mud of the present invention has peak characteristics unique to modified red mud that dry red mud does not have when performing X-ray diffraction (XRD) analysis. Specifically, the intensity of the first peak of the modified red mud at a 2θ diffraction angle of 14±0.1° is higher than the intensity of the second peak at a 2θ diffraction angle of 14.5±0.1°, which can show an excellent chlorine adsorption effect.
[0035] In one embodiment, the ratio (I1) / (I2) of the intensity of the first peak (I1) to the intensity of the second peak (I2) may be 5 or more. When (I1) / (I2) satisfies the above range, the pyrolysis efficiency and the chlorine adsorption effect may be significantly excellent, and preferably, when (I1) / (I2) is 7 or more, the chlorine adsorption effect may be more excellent. When (I1) / (I2) is 10 or more, the modified red mud exhibits uniform dispersibility with the waste plastic, and thus the heat conduction to the waste plastic is uniform, thereby increasing the yield of the pyrolysis oil, which may be more preferred. Without limitation, (I1) / (I2) may be 30 or less.
[0036] Modified red mud can be obtained by modifying ordinary red mud to meet the above peak ratio. As a specific example, the modified red mud meeting the above peak ratio can be prepared by pressurizing ordinary red mud in an atmosphere containing water vapor or pressurizing ordinary red mud in an atmosphere containing polar alcohol, but this is only an example and the present invention is not limited thereto. Any method can be used to modify ordinary red mud to meet the above peak ratio without limitation.
[0037] In one embodiment, when the modified red mud is subjected to X-ray diffraction (XRD) analysis, the intensity of the first peak having a 2θ diffraction angle of 14±0.1° may be higher than the intensity of the third peak having a 2θ diffraction angle of 28.2±0.1°.
[0038] In one embodiment, the ratio (I1) / (I3) of the intensity of the first peak (I1) to the intensity of the third peak (I3) may be 5 or more. When the intensity of the first peak having a 2θ diffraction angle of 14±0.1° is higher than the intensity of the third peak having a 2θ diffraction angle of 28.2±0.1°, especially when the ratio (I1) / (I3) of the intensity of the first peak (I1) to the intensity of the third peak (I3) is 5 or more, the selectivity for chlorine and the chlorine adsorption characteristics in the pyrolysis process may be more excellent. Specifically, (I1) / (I3) may be 7 or more. More specifically, (I1) / (I3) may be 10 or more, and may be 30 or less, without limitation.
[0039] When the modified red mud is subjected to X-ray diffraction (XRD) analysis, the chlorine adsorption effect can be maximized when the peak intensity simultaneously satisfies (I1) / (I2) being greater than 5 and (I1) / (I3) being greater than 5. That is, the modified red mud that satisfies all the above peak characteristics has a significantly higher chlorine adsorption rate, and therefore, when the waste plastic pyrolysis process is carried out in the presence of the modified red mud, high-quality pyrolysis oil with minimal impurities can be recovered. Even a simple process of pyrolysis by contacting the waste plastic raw material to be treated with the modified red mud can produce high-quality pyrolysis oil, and because the modified red mud has an excellent chlorine adsorption rate, the amount of modified red mud can be reduced compared with the adsorbent of the related art, thereby reducing the process cost and improving energy efficiency. In addition, considering that environmental pollution is caused by plastic waste and red mud waste, it is necessary to reuse these wastes. Since both types of waste are utilized, resources can be effectively recovered while effectively producing high-value-added petroleum.
[0040] In one embodiment, in the first step, the modified red mud can be loaded into the reactor in an amount of 5-30 parts by weight relative to 100 parts by weight of the waste plastic raw material. Within the above range, chlorine can be effectively adsorbed, the pyrolysis efficiency can be improved, and high-quality pyrolysis oil can be obtained. Specifically, the modified red mud can be loaded in an amount of 5-25 parts by weight, more specifically, 5-20 parts by weight relative to 100 parts by weight of the waste plastic raw material.
[0041] In one embodiment, in the first step, the modified red mud can be loaded into the reactor in a paste form by further containing water, and the content of water is 30-80 parts by weight relative to 100 parts by weight of the modified red mud. In the case where the modified red mud further contains water in the above range and is loaded into the reactor in a paste form, in the pyrolysis process, the chlorine dissociated from the waste plastic will be trapped by the water, thereby obtaining an additional chlorine adsorption effect. Specifically, relative to the total weight of the modified red mud, water can be included in an amount of 30% to 60%.
[0042] The thermal process in the second decomposition step can be carried out in the following non-oxidizing atmosphere. When the water content of the modified red mud is within the above range, the non-oxidizing atmosphere can be achieved by using the water vapor evaporated from the water content in the red mud. The problems of calcination, drying, grinding, expensive equipment, expensive processing costs, etc. in the process of using red mud in the related art can be solved, and the processing efficiency can also be improved.
[0043] In one embodiment, the second step can be carried out at a temperature of 300-600° C. Within the above range, the fusion of chlorine-containing waste plastics can be prevented, and the adsorption efficiency of chlorine dissociated from the waste plastics on the modified red mud can be improved. Specifically, the temperature can be 300-550° C., more specifically, 350-500° C.
[0044] In one embodiment, the second step can be carried out in a non-oxidizing atmosphere. A non-oxidizing atmosphere is an atmosphere in which the waste plastic will not burn, for example, an atmosphere in which the oxygen concentration is adjusted to less than 1% by volume, or an atmosphere of an inert gas such as nitrogen, water vapor, carbon dioxide or argon. The pyrolysis process can be stably carried out in a low oxygen atmosphere, in which the oxygen concentration is adjusted to less than 1% by volume.
[0045] As described above, when the modified red mud contains moisture within the above range, the non-oxidizing atmosphere can be a water vapor atmosphere evaporated from the moisture contained in the red mud. Specifically, a melting process can be performed before the pyrolysis process to improve the reaction efficiency. A process in which the waste plastic raw material and the modified red mud are loaded into a reactor and then uniformly melted at a temperature of 100-130°C for 1-2 hours can be performed. In this process, the moisture contained in the modified red mud will produce water vapor, and oxygen can be removed by pressure purging (pressure purging) performed by water vapor. That is, since the water vapor generated by the moisture contained in the raw material can form a non-oxidizing atmosphere, an additional inert gas purge process (inert gas purge process) can be omitted.
[0046] The second step can be carried out in a non-oxidizing atmosphere for 150-350 minutes. When the holding time meets the requirements, the components in the non-oxidizing atmosphere can be activated and fully pyrolyzed. Specifically, the holding time can be 170-330 minutes, more specifically, 200-300 minutes.
[0047] The reactor may be a batch reactor or a continuous reactor. In the case of a batch reactor, any type of batch reactor capable of stirring and controlling temperature rise may be used, for example, a rotary kiln type batch reactor may be selected. Among continuous reactors, a fixed bed continuous reactor may be exemplified.
[0048] When the modified red mud is dispersed in water, the pH value of the modified red mud dispersion aqueous solution can be 8-13. The strongly alkaline modified red mud meeting the above range can effectively absorb the chlorine dissociated from the waste plastic. Specifically, the pH value can be 9-12.
[0049] The modified red mud may further contain inorganic components within a certain range, wherein the sum of the components is 100 wt%. Specifically, the modified red mud may further contain at least two or more components selected from 10-30 wt% of Fe2O3, 5-20 wt% of Al2O3, 1-30 wt% of SiO2, 0-15 wt% of CaO, 1-25 wt% of TiO2 and 0-15 wt% of Na2O. More specifically, the modified red mud may further contain at least two or more components selected from 10-25 wt% of Fe2O3, 5-15 wt% of Al2O3, 1-25 wt% of SiO 2 , 0-10 wt% CaO, 1-20 wt% TiO2 and 0-10 wt% Na 2 The ingredients of O.
[0050] The first step can be carried out by further adding an admixture. An admixture within a certain range can be used to improve the efficiency of the pyrolysis reaction of waste plastics, within which the inherent physical properties of the modified red mud, especially the XRD peak characteristics, are not affected. With the further addition of the admixture, the modified red mud can be more easily mixed with the waste plastic raw material, and the long-term dispersion stability can also be improved. For example, the admixture can be, for example, a cellulose ether-based compound such as methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose or carboxymethyl cellulose. Relative to 100 parts by weight of the modified red mud, the content of the admixture can be 0.01-5 parts by weight, specifically, 0.01-3 parts by weight.
[0051] The pyrolysis reaction can be carried out by further loading an additive into the reactor. For example, the pyrolysis process is carried out by further adding one or more dechlorinating agents selected from metal oxides, metal hydroxides and metal carbonates, so as to further improve the adsorption effect of chlorine. The metal can be an alkali metal or an alkaline earth metal, specifically, sodium, magnesium, potassium, calcium, etc., and more specifically, the dechlorinating agent can be calcium hydroxide, sodium hydroxide, magnesium hydroxide, potassium hydroxide, calcium oxide, magnesium oxide, calcium carbonate, sodium carbonate, potassium carbonate, etc. Relative to 100 parts by weight of the waste plastic raw material, the dechlorinating agent can be added in an amount of 1-10 parts by weight. Specifically, the dechlorinating agent can be added in an amount of 1-5 parts by weight. In addition, additives such as stabilizers, defoamers and dispersants can also be added.
[0052] The waste plastic raw material may be household waste plastic, industrial waste plastic or mixed waste plastic thereof. Household waste plastic refers to plastics mixed with PVC, PS, PET, PBT, etc. in addition to PE and PP. In the present invention, as an example, household waste plastic may be waste plastic including more than 3 wt% PVC, as well as PE and PP. The chlorine content may be more than 5,000 ppm relative to 100 parts by weight of household waste plastic, specifically, the chlorine content may be 5,000-15,000 ppm relative to 100 parts by weight of household waste plastic, but this is only an example and the present invention is not limited thereto.
[0053] Industrial waste plastics are industrial wastes generated in industrial production processes, and may be waste plastics including PE and PP as main components. Since industrial waste plastics remain in a relatively clean state, the chlorine content is lower than that in domestic waste plastics. However, the organic chlorine content from adhesives or dye components is high, especially the proportion of chlorine contained in aromatic rings is high. Relative to 100 parts by weight of waste plastics, the chlorine content may be 100-1000ppm, specifically, 500-1000ppm, more specifically, 700-1000ppm, but the present invention is not limited thereto.
[0054] The second step is to pyrolyze the waste plastic raw material and recover the pyrolysis oil. The waste plastic raw material is converted into hydrocarbon compound products and may contain pyrolysis gas. After the pyrolysis gas is discharged from the reactor, the pyrolysis gas can be cooled and liquefied in a condenser to recover liquid pyrolysis oil in a storage tank.
[0055] Relative to the total weight of the waste plastic raw materials, the pyrolysis gas may include 5-35 wt % of naphtha (boiling point (bp) below 150°C), 10-60 wt % of kerosene (Kero) (boiling point 150-265°C), 20-40 wt % of light gas oil (LGO) (boiling point 265-380°C) and 5-40 wt % of UCO-2 / AR (boiling point above 380°C). Specifically, relative to the total weight of the waste plastic raw materials, it may include 5-30 wt % of naphtha (boiling point below 150°C), 15-50 wt % of kerosene (boiling point 150-265°C), 20-35 wt % of LGO (boiling point 265-380°C) and 10-40 wt % of UCO-2 / AR (boiling point above 380°C). In addition, the pyrolysis gas may include a residual amount of low-boiling hydrocarbon compounds, such as methane (CH4), ethane (C2H6) and propane (C3H8).
[0056] Before the pyrolysis gas is introduced into the condenser, low boiling point gases containing low boiling point hydrocarbon compounds such as methane (CH4), ethane (C2H6) and propane (C3H8) in the pyrolysis gas can be recovered separately. The pyrolysis gas generally contains combustible substances such as hydrogen, carbon monoxide and low molecular weight hydrocarbon compounds. Examples of hydrocarbon compounds include methane, ethane, ethylene, propane, propylene, butane and butene. Since the pyrolysis gas contains combustible substances, the pyrolysis gas can be reused as a fuel for heating a batch reactor or a continuous reactor.
[0057] The condenser may include a region through which a coolant flows, and the pyrolysis gas introduced into the condenser may be liquefied by the coolant and converted into pyrolysis oil. When the pyrolysis oil generated in the condenser rises to a predetermined level, the pyrolysis oil may be transported to a storage tank and recovered.
[0058] A heat exchanger may be further arranged between the condenser and the storage tank. The uncondensed pyrolysis gas in the condenser is introduced into the heat exchanger and condensed again, and the generated pyrolysis oil can be recycled into the storage tank. The uncondensed pyrolysis gas is recycled again, thereby improving the reaction yield.
[0059] The liquid pyrolysis oil recovered in the storage tank may include an oil layer and a water layer. In addition to the pyrolysis gas, the water vapor generated by the modified red mud is also liquefied and recovered in the storage tank, and oil-water separation is performed to form an oil layer and a water layer in the liquid pyrolysis oil.
[0060] The water layer contains chlorine compounds, which may corrode the storage tank, so a neutralizer can be added to the water layer to prevent the storage tank from being corroded. The neutralizer may include an alkali metal compound or an alkaline earth metal compound having a pH value of more than 7 when dissolved in water. Specifically, the neutralizer may contain hydroxides, oxides, carbonates, bicarbonates, basic carbonates or fatty acid salts of alkali metals or alkaline earth metals. Alkali metals or alkaline earth metals may be metals commonly used in the art. Examples of alkali metals include lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs) and francium (Fr), and examples of alkaline earth metals include beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba) and radium (Ra). The neutralizer may be added alone, or may be mixed with a solvent such as an alcohol to improve the neutralization efficiency.
[0061] In the case where the neutralizing agent is added to the water layer, the neutralizing agent may be added in an appropriate amount by measuring the pH value of the water layer using a pH meter located at the bottom of the storage tank.
[0062] When the oil layer and the water layer are separated, the oil layer can be recovered immediately, or after the water layer is adsorbed, so that the oil layer (waste plastic pyrolysis oil) with the minimum chlorine content can be recovered. The water layer can be discharged and adsorbed, and the discharged water can be purified and then recycled to the first step as water mixed with waste plastics.
[0063] An electric field can be applied to effectively separate the oil layer and the water layer. Due to the application of the electric field, the oil layer and the water layer can be separated in a short time by electrostatic adhesion. In addition, additives can be added as needed to improve the oil-water separation efficiency. The additives can be conventional demulsifiers known in the art.
[0064] In the case where the water layer is discharged and adsorbed, a density profiler is used to detect the density, which can prevent the oil layer from being adsorbed together with the water layer when the water layer is adsorbed, and only the water layer can be effectively removed.
[0065] The chlorine content in the recovered pyrolysis oil can be less than 300 ppm. The chlorine content in the produced pyrolysis oil of waste plastics can be less than 300 ppm by effectively adsorbing the chlorine dissociated from the waste plastic raw material by using modified red mud. In particular, when the relationship 1(I 1D / I 1W ) / (I 2D / I 2W ) and relation 2(I 2W / I 1W ) are all satisfied, the adsorption effect of chlorine is maximized, so the chlorine content can be below 150 ppm, more specifically, below 100 ppm.
[0066] Preferred embodiments and comparative examples of the present invention will be described below. However, the following embodiments are merely preferred embodiments of the present invention, and the present invention is not limited to the following embodiments.
[0067] Example 1
[0068] A household mixed plastic including more than 3 wt % of PVC, and PE and PP was extruded at 250° C. to prepare 400 g of household waste plastic pellets. The total chlorine content in the household waste plastic pellets was 4,000 ppm.
[0069] The common red mud recovered from the residue after preparing alumina from bauxite was prepared. The composition of the recovered common red mud is shown in Table 1.
[0070] Table 1
[0071]
[0072] Ordinary red mud is added to a pressurizing device in which a water vapor atmosphere is formed, and pressurized for 60 minutes at a pressure of 5 bar and a temperature of 25°C. Then, the pressure is adjusted to normal pressure and stabilized at a temperature of 60°C for 60 minutes to prepare modified red mud. 400g of prepared household waste plastic particles and 20g of modified red mud are added to an intermittent reactor, heated at a temperature of 110°C for 1 hour, and melted. The water vapor generated by the modified red mud in the melting process is used to create a non-oxidizing atmosphere, and then full-scale pyrolysis is performed at 400°C for 250 minutes. The pyrolysis gas generated in the pyrolysis process is recovered through the outlet at the top of the reactor and captured by the condenser, and finally the waste plastic pyrolysis oil is recovered in the storage tank.
[0073] X-ray diffraction (XRD) analysis was performed to confirm the peak characteristics of the modified red mud. The results are shown in Table 2. I1, I2 and I3 in the following table have the same definitions as above.
[0074] Table 2
[0075]
[0076] Example 2
[0077] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that the modified red mud having the characteristics shown in Table 3 was used. Specifically, ordinary red mud was added to a pressurizing device in which a water vapor atmosphere was formed, and pressurized for 60 minutes under the conditions of a pressure of 7 bar and a temperature of 25° C., thereby preparing modified red mud.
[0078] Table 3
[0079]
[0080] Example 3
[0081] In Example 1, ordinary red mud having the composition shown in Table 4 was used instead of ordinary red mud having the composition shown in Table 1, and was added to a pressurizing device for forming an ethanol atmosphere, and pressurized for 60 minutes at a pressure of 5 bar and a temperature of 25°C.
[0082] Table 4
[0083]
[0084] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that modified red mud having the properties shown in Table 5 was prepared and used.
[0085] Table 5
[0086]
[0087] Example 4
[0088] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that modified red mud having the characteristics shown in Table 6 was used in Example 4. Specifically, ordinary red mud was added to a pressurizing device for forming an ethanol atmosphere, and pressurized for 60 minutes under the conditions of a pressure of 15 bar and a temperature of 25° C., thereby preparing modified red mud.
[0089] Table 6
[0090]
[0091] Comparative Example 1
[0092] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that dry red mud obtained by drying ordinary red mud was used. Specifically, the modified red mud was heated at 110° C. for 24 hours to prepare dry red mud.
[0093] X-ray diffraction (XRD) analysis was performed to confirm the peak characteristics of the dried red mud. Figure 1 And as shown in Table 7.
[0094] Table 7
[0095]
[0096] Comparative Example 2
[0097] The reaction was carried out under the same conditions as in Example 1 to recover the waste plastic pyrolysis oil, except that red mud having the properties shown in Table 8 was used.
[0098] Table 8
[0099]
[0100] Evaluation Example 1
[0101] Representatively, each of the red muds in Example 3 and Comparative Example 1 was subjected to X-ray diffraction (XRD) analysis to measure the peak intensities at 2θ diffraction angles of 14±0.1°, 14.5±0.1°, and 28.2±0.1°. The measurement results are shown in Table 9.
[0102] Table 9
[0103]
[0104] Refer to Table 9 and Figure 1, it can be determined that I1 in Example 3 is higher than I2, while I1 in Comparative Example 1 is lower than I2, and it can be determined that I3 in Example 3 is lower than I3 in Comparative Example 2. It can be confirmed that in Example 3, each of (I1) / (I2) and (I1) / (I3) satisfies 5 or more, while it is not satisfied in Comparative Example 1, and it can be confirmed that the chlorine removal characteristics of red mud are different due to the difference in peak characteristics, as shown in Table 10 described below.
[0105] Evaluation Example 2
[0106] ICP and XRF analysis were performed on the recycled waste plastic pyrolysis oil to measure the chlorine content. The results are summarized in Table 10.
[0107] Table 10
[0108]
[0109] In Examples 1 and 2, it was confirmed that the chlorine content in the recovered pyrolysis oil was about 250-270 ppm due to the (I1) / (I2) values of the modified red mud being 7.38 and 9.92 (satisfying 5 or more), respectively, indicating that chlorine was effectively reduced. In particular, with reference to Examples 3 and 4, it was confirmed that the chlorine content in the pyrolysis oil was 200 ppm or less when the (I1) / (I2) values were 11.74 and 13.89 (satisfying 5 or more), and the (I1) / (I3) values were 12.51 and 17.64 (satisfying 5 or more), respectively, indicating that the chlorine removal properties of the modified red mud were further improved.
[0110] On the other hand, it can be confirmed that in the case of the conventional dry red mud of Comparative Example 1, the (I1) / (I2) value is less than 1, and the (I1) / (I3) value is less than 3, which are significantly low values. Therefore, it can be confirmed that the chlorine removal characteristics of the modified red mud are deteriorated, and the chlorine content in the pyrolysis oil is 530 ppm, which indicates that there is an excess of chlorine.
[0111] Also in Comparative Example 2, since the (I1) / (I2) value is 1 or less and the (I1) / (I3) value is 5 or less, both values are low, it can be confirmed that the chlorine removal property of the modified red mud is deteriorated.
[0112] Although the embodiments of the present invention have been described above, the present invention is not limited to the embodiments, but can be implemented in various forms. It is obvious to those skilled in the art that the embodiments of the present invention can be implemented in other specific forms without departing from the technical ideas or basic features of the present invention. Therefore, it should be understood that the embodiments described herein are illustrative in all aspects and not restrictive.
Claims
1. A method for producing pyrolysis oil of waste plastics with reduced chlorine content, the method comprising The first step is to load the waste plastic feedstock and modified red mud into the reactor; and The second step is to pyrolyze the waste plastic raw material in a reactor and recover the pyrolysis oil, in, When the modified red mud is subjected to X-ray diffraction (XRD) analysis, the intensity of the first peak having a 2θ diffraction angle of 14±0.1° is higher than the intensity of the second peak having a 2θ diffraction angle of 14.5±0.1°.
2. The method according to claim 1, wherein the intensity of the first peak (I 1 ) and the intensity of the second peak (I 2 ) ratio (I 1 ) / (I 2 ) is 5 or more.
3. The method according to claim 1, wherein when the modified red mud is subjected to X-ray diffraction (XRD) analysis, the intensity of the first peak having a 2θ diffraction angle of 14±0.1° is higher than the intensity of the third peak having a 2θ diffraction angle of 28.2±0.1°.
4. The method according to claim 1, wherein the intensity of the first peak (I 1 ) and the intensity of the third peak (I 3 ) ratio (I 1 ) / (I 3 ) is 5 or more.
5. The method according to claim 1, wherein in the first step, the modified red mud is charged into the reactor in an amount of 5-30 parts by weight relative to 100 parts by weight of the waste plastic raw material.
6. The method according to claim 1, wherein in the first step, the modified red mud is charged into the reactor in a paste form by further containing moisture, and the amount of the moisture is 30-80 parts by weight relative to 100 parts by weight of the modified red mud.
7. The method according to claim 1, wherein the second step is performed at a temperature of 300-600°C.
8. The method according to claim 1, wherein the second step is performed in a non-oxidizing atmosphere.
9. The method according to claim 1, wherein the first step is performed by further containing a blending agent.
10. The method according to claim 9, wherein the admixture is a cellulose ether-based compound.
Citation Information
Cited By
Refining and separating process of catalytic slurry oil