Strontium-containing calcium sulfate compound feed additive and preparation method thereof

Prepare strontium calcium sulfate through hydrothermal method and coat the material on its surface, solving the problems of low bioavailability of strontium element and insufficient solubility of calcium sulfate, achieving sustained release of strontium and calcium elements, avoiding poisoning and promoting bone health and nutrition absorb.

CN118901912AActive Publication Date: 2024-11-08SICHUAN ZIGONG CHI YU SALT PROD CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411074625.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-08
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The bioavailability of strontium in existing animal feed is low and easy to cause poisoning reactions. Calcium sulfate is not solubility in the gastrointestinal tract, which affects nutrient absorption.

Method used

Strontium calcium sulfate was prepared by hydrothermal method and coated with carboxymethyl chitosan and hyaluronic acid on its surface. N-acetylcysteine ​​activation was used to improve the sustained release performance of strontium calcium sulfate and slow down strontium and calcium Breaking release of elements.

Benefits of technology

It improves the sustained release properties of strontium and calcium, avoids the poisoning reaction caused by excessive release, and promotes bone health and nutritional absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901912A_ABST
    Figure CN118901912A_ABST
Patent Text Reader

Abstract

The invention discloses a compound feed additive containing strontium calcium sulfate and a preparation method of the compound feed additive in the field of feed additives. The compound feed additive is prepared from the following raw materials in parts by weight: 5-10 parts of strontium calcium sulfate, 1-2 parts of carboxymethyl chitosan and 0.1-0.2 part of hyaluronic acid. Strontium chloride and calcium chloride are used as raw materials to prepare strontium calcium sulfate through a hydrothermal method, N-acetylcysteine is adopted to activate the strontium calcium sulfate, carboxymethyl chitosan and hyaluronic acid are coated on the surface of the strontium calcium sulfate, and the slow release performance of the strontium calcium sulfate is improved, so that burst release of strontium element and calcium element in the feed is slowed down; the poisoning reaction on the body caused by excessive release of the strontium element and the calcium element is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of feed additives, and specifically refers to a composite feed additive containing strontium and calcium sulfate and a preparation method thereof. Background Art

[0002] Calcium sulfate, commonly known as gypsum, usually exists in the form of calcium sulfate dihydrate. It can be used as an additive such as a binder, anti-caking agent, stabilizer and emulsifier in animal feed and breeding processes for ruminants, poultry, aquatic products, etc. It has been officially included in the "Catalogue of Feed Additives (2023)" announced by the Ministry of Agriculture and Rural Affairs, and is especially widely used in pet feed. After being digested and decomposed by animals, calcium sulfate can provide calcium and sulfur elements. Calcium is one of the essential mineral elements for animals. The solubility of calcium sulfate in the gastrointestinal environment is not high, but it can dissolve slowly to provide free calcium ions. After calcium sulfate is completely dissolved, the calcium ion aqueous solution is the main solution, which is less irritating to the gastrointestinal environment and is conducive to the full absorption of nutrients. Calcium sulfate It can provide sulfur, which is beneficial for the synthesis of cystine, cysteine ​​and methionine in animals. It is also a component of heparin, taurine and bile, and plays an important role in the body's detoxification process. Strontium has active chemical properties and easily reacts with oxygen and water. It mainly exists in the form of strontium sulfate and strontium carbonate in nature, and mainly exists in the form of strontium ions in animals. Strontium can promote bone health, increase bone density, promote bone formation and bone absorption, regulate reproductive health, and improve the success rate of fertilization and the live birth rate. Strontium also has the effect of improving immunity. Strontium in animal feed often exists in the form of strontium perchlorate and strontium chloride, but its bioavailability is low, and adding excessive strontium can easily cause poisoning reactions. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a composite feed additive containing strontium calcium sulfate and a preparation method thereof. The present invention prepares strontium calcium sulfate using strontium chloride and calcium chloride as raw materials through a hydrothermal method, activates the strontium calcium sulfate with N-acetylcysteine, and coats carboxymethyl chitosan and hyaluronic acid on its surface to improve the sustained-release performance of the strontium calcium sulfate, thereby slowing down the sudden release of strontium and calcium elements in the feed, and avoiding poisoning reactions caused by excessive release of strontium and calcium elements to the body.

[0004] In order to achieve the above object, the technical scheme adopted by the present invention is as follows: the present invention proposes a composite feed additive containing strontium calcium sulfate, the raw materials for preparing the composite feed additive include the following components in parts by weight: 5-10 parts of strontium calcium sulfate, 1-2 parts of carboxymethyl chitosan, and 0.1-0.2 parts of hyaluronic acid;

[0005] Preferably, the preparation method of strontium calcium sulfate specifically comprises the following steps:

[0006] S1, dissolving strontium chloride and calcium chloride in deionized water, adding sodium sulfate after mixing evenly, stirring at a speed of 200-220rpm for 30-40min, adjusting the pH to 4-5, and obtaining a strontium calcium sulfate precursor solution;

[0007] Preferably, in step S1, the raw materials for preparing the strontium calcium sulfate precursor solution are the following components in parts by weight: 0.15-0.6 parts of strontium chloride, 0.9-1 parts of calcium chloride, and 1.4-1.8 parts of sodium sulfate;

[0008] S2, raising the temperature of the strontium calcium sulfate precursor solution prepared in step S1 to 110-120°C, hydrothermally reacting for 2-2.5 hours, then lowering the temperature of the reaction system to 100°C, filtering, washing the precipitate with boiling water and anhydrous ethanol, drying in an oven to obtain strontium calcium sulfate, grinding, passing through a 300-mesh sieve, and setting aside;

[0009] The present invention also provides a method for preparing a composite feed additive containing strontium and calcium sulfate, which specifically comprises the following steps:

[0010] ① Place strontium calcium sulfate in a beaker, add deionized water to disperse, add N-acetylcysteine ​​and mix well, raise the reaction temperature to 80-90°C, stir the reaction at 400-500rpm for 4-6h, centrifuge at 5000rpm for 20min, collect the precipitate, disperse it in a sodium hydroxide solution, maintain the reaction temperature at 30-35°C, and the reaction time is 30-40min. After the reaction system is cooled to room temperature, filter and collect the precipitate to obtain activated strontium calcium sulfate;

[0011] Preferably, in step ①, the mass ratio between the strontium calcium sulfate and N-acetylcysteine ​​is 4:1-2;

[0012] Preferably, in step ①, the mass concentration of sodium hydroxide in the sodium hydroxide solution is 5-10 g / L, and the mass volume ratio g / mL between strontium calcium sulfate and the sodium hydroxide solution is 0.06-0.08 g / mL;

[0013] ② Place carboxymethyl chitosan in deionized water, disperse and mix evenly with ultrasonic dispersion, add EDC and NHS, stir at 450-500 rpm for 4-5 hours at room temperature, add activated strontium calcium sulfate prepared in step ①, continue stirring for 10-12 hours, after the reaction is completed, centrifuge at 5000 rpm for 10 minutes, collect the precipitate, and dry in vacuum to obtain carboxymethyl chitosan modified strontium calcium sulfate;

[0014] Preferably, in step ②, the mass ratio of EDC to carboxymethyl chitosan is 2.5-3:1, and the mass ratio of NHS to carboxymethyl chitosan is 1.5-2:1;

[0015] ③ Disperse hyaluronic acid in deionized water, add the carboxymethyl chitosan modified strontium calcium sulfate prepared in step ②, add EDC and NHS, stir and react at 500-550 rpm, centrifuge at 5000 rpm for 15 min after 20-24 h, collect the precipitate, and freeze-dry to obtain modified strontium calcium sulfate powder;

[0016] Preferably, in step ③, the mass ratio of EDC to hyaluronic acid is 4-5:1, and the mass ratio of NHS to hyaluronic acid is 2.5-3:1;

[0017] ④ Mix the modified strontium calcium sulfate prepared in step ③ with deionized water and inject into a mold with mold parameters of 10 mm in diameter and 3 mm in height. After curing, a composite feed additive is obtained;

[0018] Preferably, in step ④, the mass volume ratio between the modified strontium calcium sulfate and deionized water is 1-1.5 g / mL.

[0019] The beneficial effects achieved by the present invention are as follows:

[0020] The invention provides a composite feed additive containing strontium calcium sulfate and a preparation method thereof. The invention uses a hydrothermal method to prepare strontium calcium sulfate using strontium chloride and calcium chloride as raw materials, uses N-acetylcysteine ​​to activate the calcium sulfate, and coats carboxymethyl chitosan and hyaluronic acid on the surface of the calcium sulfate to improve the sustained-release performance of the calcium sulfate, thereby slowing down the sudden release of strontium and calcium elements in the feed, and avoiding poisoning reactions caused by excessive release of strontium and calcium elements to the body; the invention uses N-acetylcysteine ​​to bind calcium ions and strontium ions through carboxyl groups. The electrostatic force between them is used to connect N-acetylcysteine ​​and calcium strontium sulfate, and deacetylation is carried out through a mild alkaline hydrolysis reaction to obtain calcium strontium sulfate with amino active groups; carboxymethyl chitosan is coated on the surface of calcium strontium sulfate through the hydrogen bonding between the amino group and carboxymethyl chitosan. The swelling properties of hyaluronic acid are different under different pH conditions, resulting in different release rates of calcium ions and strontium ions, thereby improving the sustained release performance of the composite feed additive for strontium ions and calcium ions and avoiding excessive absorption of calcium ions and strontium ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM image of the composite feed additive prepared in Example 1 of the present invention;

[0022] Figure 2The feed additive Ca prepared in Examples 1-3 and Comparative Examples 1-2 2+ Release result diagram;

[0023] Figure 3 The feed additive Sr prepared in Examples 1-3 and Comparative Examples 1-2 2+ Release result diagram;

[0024] Figure 4 The Ca content of the feed additives prepared in Examples 1-3 and Comparative Examples 1-2 under different pH conditions 2+ Release the result graph.

[0025] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0028] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.

[0029] Example 1

[0030] This embodiment provides a composite feed additive containing strontium calcium sulfate and a preparation method thereof. The raw materials for preparing the composite feed additive include the following components in parts by weight: 5 parts of strontium calcium sulfate, 2 parts of carboxymethyl chitosan, and 0.1 parts of hyaluronic acid;

[0031] The preparation method of strontium calcium sulfate specifically comprises the following steps:

[0032] S1. Accurately weigh 0.15 g of strontium chloride and 1 g of calcium tetrachloride dihydrate into a beaker, add 100 mL of deionized water, mix well, accurately weigh 1.4 g of sodium sulfate and add it to the reaction system, stir at 220 rpm for 30 min, and adjust the pH to 5 with 0.1 mol / L hydrochloric acid solution to obtain a strontium calcium sulfate precursor solution;

[0033] S2, raising the temperature of the strontium calcium sulfate precursor solution prepared in step S1 to 110-120°C, hydrothermally reacting for 2-2.5 hours, then lowering the temperature of the reaction system to 100°C, filtering, washing the precipitate with boiling water and anhydrous ethanol, drying in an oven to obtain strontium calcium sulfate, grinding, passing through a 300-mesh sieve, and setting aside;

[0034] This embodiment also provides a method for preparing a strontium calcium sulfate composite feed additive, which specifically comprises the following steps:

[0035] ① Accurately weigh 4 g of strontium calcium sulfate and place it in a beaker, add 50 mL of deionized water to the beaker, place the strontium calcium sulfate under 400 W for ultrasonic dispersion, add 1 g of N-acetylcysteine ​​and continue ultrasonic dispersion. After uniform dispersion, increase the reaction temperature to 90 ° C, stir the reaction at 400 rpm for 5 hours, and after the reaction is cooled to room temperature, place it at 5000 rpm for centrifugation for 20 minutes, collect the precipitate and disperse it in 50 mL of sodium hydroxide solution with a mass concentration of 5 g / mL, increase the reaction temperature to 35 ° C, react for 30 minutes, and after the reaction system is cooled to room temperature, filter, collect the precipitate, and place it at 25 ° C for vacuum drying to obtain activated strontium calcium sulfate;

[0036] ② Accurately weigh 1.6 g of carboxymethyl chitosan and disperse it in 100 mL of deionized water, place it under 400 W power for ultrasonic dispersion, and after uniform dispersion, add 4 g of EDC and 2.4 g of NHS, place it at 500 rpm and stir for 5 h, add the activated strontium calcium sulfate prepared in step ①, continue stirring for 12 h, after the reaction is completed, centrifuge at 5000 rpm for 10 min, collect the precipitate, and vacuum dry it at 25 ° C to obtain carboxymethyl chitosan modified strontium calcium sulfate;

[0037] ③ Accurately weigh 0.08 g of hyaluronic acid and disperse it in 50 mL of deionized water. After uniform dispersion, add the carboxymethyl chitosan modified strontium calcium sulfate prepared in step ② and place it under 400 W for ultrasonic dispersion. Add 0.4 g of EDC and 0.2 g of NHS, stir and react at 550 rpm for 20 h, centrifuge at 5000 rpm for 15 min, collect the precipitate, and obtain modified strontium calcium sulfate powder after freeze-drying;

[0038] ④ Take 5 g of the modified strontium calcium sulfate prepared in step ③, mix it with 5 mL of deionized water to form a paste, inject it into a polytetrafluoroethylene mold with a diameter of 10 mm and a height of 3 mm, and after curing, obtain a composite feed additive.

[0039] Example 2

[0040] This embodiment provides a composite feed additive containing strontium calcium sulfate and a preparation method thereof. The raw materials for preparing the composite feed additive include the following components in parts by weight: 8 parts of strontium calcium sulfate, 1.5 parts of carboxymethyl chitosan, and 0.15 parts of hyaluronic acid;

[0041] The preparation method of strontium calcium sulfate specifically comprises the following steps:

[0042] S1. Accurately weigh 0.3 g of strontium chloride and 0.9 g of calcium tetrachloride dihydrate into a beaker, add 100 mL of deionized water, mix well, accurately weigh 1.4 g of sodium sulfate and add it to the reaction system, stir at 200 rpm for 40 min, and adjust the pH to 4.5 with 0.1 mol / L hydrochloric acid solution to obtain a strontium calcium sulfate precursor solution;

[0043] S2, raising the temperature of the strontium calcium sulfate precursor solution prepared in step S1 to 110-120°C, hydrothermally reacting for 2-2.5 hours, then lowering the temperature of the reaction system to 100°C, filtering, washing the precipitate with boiling water and anhydrous ethanol, drying in an oven to obtain strontium calcium sulfate, grinding, passing through a 300-mesh sieve, and setting aside;

[0044] This embodiment also provides a method for preparing a composite feed additive containing strontium and calcium sulfate, which specifically comprises the following steps:

[0045] ① Accurately weigh 4 g of strontium calcium sulfate and place it in a beaker, add 50 mL of deionized water to the beaker, place the strontium calcium sulfate under 400 W for ultrasonic dispersion, add 2 g of N-acetylcysteine ​​and continue ultrasonic dispersion. After uniform dispersion, increase the reaction temperature to 80 ° C, stir at 500 rpm for 4 hours, wait for the reaction to cool to room temperature, place it at 5000 rpm for centrifugation for 20 minutes, collect the precipitate and disperse it in 70 mL of sodium hydroxide solution with a mass concentration of 7.5 g / mL, increase the reaction temperature to 30 ° C, react for 30 minutes, wait for the reaction system to cool to room temperature, filter, collect the precipitate, and place it at 25 ° C for vacuum drying to obtain activated strontium calcium sulfate;

[0046] ② Accurately weigh 0.75g of carboxymethyl chitosan and disperse it in 100mL of deionized water, place it under 400W power for ultrasonic dispersion, and after uniform dispersion, add 2.25g of EDC and 1.5g of NHS, stir and react at 500rpm for 4h, add the activated strontium calcium sulfate prepared in step ①, continue stirring for 10h, after the reaction is completed, centrifuge at 5000rpm for 10min, collect the precipitate, and vacuum dry at 25°C to obtain carboxymethyl chitosan modified strontium calcium sulfate;

[0047] ③ Accurately weigh 0.075 g of hyaluronic acid and disperse it in 50 mL of deionized water. After uniform dispersion, add the carboxymethyl chitosan modified strontium calcium sulfate prepared in step ② and place it under 400 W for ultrasonic dispersion. Add 0.3 g of EDC and 0.2 g of NHS, stir and react at 500 rpm for 24 h, centrifuge at 5000 rpm for 15 min, collect the precipitate, and obtain modified strontium calcium sulfate powder after freeze-drying;

[0048] ④ Take 5 g of the modified strontium calcium sulfate prepared in step ③, mix it with 7.5 mL of deionized water to form a paste, inject it into a polytetrafluoroethylene mold with a diameter of 10 mm and a height of 3 mm, and after curing, obtain a composite feed additive.

[0049] Example 3

[0050] The present embodiment provides a composite feed additive containing strontium calcium sulfate and a preparation method thereof. The raw materials for preparing the composite feed additive include the following components in parts by weight: 10 parts of strontium calcium sulfate, 1 part of carboxymethyl chitosan, and 0.2 parts of hyaluronic acid;

[0051] The preparation method of strontium calcium sulfate specifically comprises the following steps:

[0052] S1. Accurately weigh 0.47 g of strontium chloride and 0.8 g of calcium tetrachloride dihydrate into a beaker, add 100 mL of deionized water, mix well, accurately weigh 1.4 g of sodium sulfate and add it to the reaction system, stir at 220 rpm for 30 min, and adjust the pH to 4 with 0.1 mol / L hydrochloric acid solution to obtain a strontium calcium sulfate precursor solution;

[0053] S2, raising the temperature of the strontium calcium sulfate precursor solution prepared in step S1 to 110-120°C, hydrothermally reacting for 2-2.5 hours, then lowering the temperature of the reaction system to 100°C, filtering, washing the precipitate with boiling water and anhydrous ethanol, drying in an oven to obtain strontium calcium sulfate, grinding, passing through a 300-mesh sieve, and setting aside;

[0054] This embodiment also provides a method for preparing a composite feed additive containing strontium and calcium sulfate, which specifically comprises the following steps:

[0055] ① Accurately weigh 4 g of strontium calcium sulfate and place it in a beaker, add 50 mL of deionized water to the beaker, place the strontium calcium sulfate under 400 W for ultrasonic dispersion, add 1.5 g of N-acetylcysteine ​​and continue ultrasonic dispersion. After uniform dispersion, increase the reaction temperature to 85 ° C, stir the reaction at 450 rpm for 6 hours, wait for the reaction to cool to room temperature, place it at 5000 rpm for centrifugation for 20 minutes, collect the precipitate and disperse it in 60 mL of sodium hydroxide solution with a mass concentration of 10 g / mL, increase the reaction temperature to 30 ° C, react for 40 minutes, wait for the reaction system to cool to room temperature, filter, collect the precipitate, and place it at 25 ° C for vacuum drying to obtain activated strontium calcium sulfate;

[0056] ② Accurately weigh 0.4 g of carboxymethyl chitosan and disperse it in 100 mL of deionized water, place it under ultrasonic dispersion at 400 W power, and after uniform dispersion, add 1 g of EDC and 0.6 g of NHS, stir and react at 450 rpm for 5 h, add the activated strontium calcium sulfate prepared in step ①, continue stirring for 12 h, and after the reaction is completed, centrifuge at 5000 rpm for 10 min, collect the precipitate, and vacuum dry it at 25 ° C to obtain carboxymethyl chitosan modified strontium calcium sulfate;

[0057] ③ Accurately weigh 0.08 g of hyaluronic acid and disperse it in 50 mL of deionized water. After uniform dispersion, add the carboxymethyl chitosan modified strontium calcium sulfate prepared in step ② and place it under 400 W for ultrasonic dispersion. Add 0.32 g of EDC and 0.24 g of NHS, stir and react at 550 rpm for 20 h, centrifuge at 5000 rpm for 15 min, collect the precipitate, and obtain modified strontium calcium sulfate powder after freeze-drying;

[0058] ④ Take 5 g of the modified strontium calcium sulfate prepared in step ③, mix it with 6 mL of deionized water to form a paste, inject it into a polytetrafluoroethylene mold with a diameter of 10 mm and a height of 3 mm, and after curing, obtain a composite feed additive.

[0059] Comparative Example 1

[0060] This comparative example provides a feed additive and a preparation method thereof, which is different from Example 1 only in that the composite feed additive does not include hyaluronic acid, and its components and component contents are the same as those in Example 1.

[0061] Comparative Example 2

[0062] This comparative example provides a feed additive and a preparation method thereof, which differs from Example 1 in that the preparation method of the composite feed additive does not include step ①, and strontium calcium sulfate is used instead of the activated strontium calcium sulfate in step ②.

[0063] Experimental Example 1

[0064] In this experimental example, the microscopic morphology of the composite feed additive prepared in Example 1 was observed and analyzed. The sample surface was brittle fractured with liquid nitrogen, and the sample surface was sprayed with gold after being thoroughly dried. Finally, the sample surface morphology was observed using a JSM-6510 scanning electron microscope.

[0065] Figure 1 This is a SEM image of the composite feed additive prepared in Example 1 of the present invention. As shown in the figure, the particles of the composite feed additive have a rough surface and an ellipsoidal shape, and the average particle size is 80-90nm.

[0066] Experimental Example 2

[0067] In this experimental example, the in vitro release performance of the feed additives prepared in Examples 1-3 and Comparative Examples 1-2 was measured. The feed additives prepared in Examples 1-3 and Comparative Examples 1-2 were dispersed in simulated body fluid at a concentration of 10 mg / mL, and the simulated body fluid was shaken at 37°C and 150 rpm. The simulated body fluid was sampled at different times, and the Ca 2+ and Sr 2+ concentration;

[0068] Figure 2 The feed additive Ca prepared in Examples 1-3 and Comparative Examples 1-2 2+ The release result diagram, Figure 3 The feed additive Sr prepared in Examples 1-3 and Comparative Examples 1-2 2+ The release result diagram is shown in the figure. The feed additives prepared in Examples 1-3 can continuously release calcium ions and strontium ions within 7 days. The feed additive prepared in Comparative Example 1 can also continuously release calcium ions and strontium ions within 7 days, but the release amount is significantly lower than that in the embodiment. The feed additive prepared in Comparative Example 2 reaches equilibrium at 4 days, and the release amount of calcium ions and strontium ions is significantly reduced within the subsequent 3 days; This shows that the feed additive prepared by the present invention can slowly release calcium ions and strontium ions in the in vivo environment.

[0069] Figure 4 The Ca content of the feed additives prepared in Examples 1-3 and Comparative Examples 1-2 under different pH conditions 2+ The release result diagram shows the release concentration of calcium ions after 7 days at pH = 5.0 and pH = 7.4 for the feed additives prepared in Examples 1-3 and Comparative Examples 1-2. It can be seen that under the condition of pH = 5, the Ca ion release concentration of the feed additives prepared in Examples 1-3 is 2+ The release concentration of the feed additive and strontium calcium sulfate under different pH conditions was significantly higher than that of pH 7.4. 2+The release concentration is the same, and the feed additive in Comparative Example 2 is 7.4 higher under pH=5.0.

[0070] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.

[0071] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A composite feed additive containing strontium and calcium sulfate, Features: The raw materials for preparing the composite feed additive include the following components in parts by weight: 5-10 parts of strontium calcium sulfate, 1-2 parts of carboxymethyl chitosan, and 0.1-0.2 parts of hyaluronic acid.

2. A composite feed additive containing strontium and calcium sulfate according to claim 1, Features: The preparation method of strontium calcium sulfate specifically comprises the following steps: S1, dissolving strontium chloride and calcium chloride in deionized water, adding sodium sulfate after mixing evenly, stirring at a speed of 200-220rpm for 30-40min, adjusting the pH to 4-5, and obtaining a strontium calcium sulfate precursor solution; S2. The temperature of the strontium calcium sulfate precursor solution prepared in step S1 is raised to 110-120° C., and after a hydrothermal reaction for 2-2.5 hours, the temperature of the reaction system is lowered to 100° C., filtered, and the precipitate is washed with boiling water and anhydrous ethanol, and placed in an oven to dry to obtain strontium calcium sulfate, which is ground and passed through a 300-mesh sieve for standby use.

3. A composite feed additive containing strontium and calcium sulfate according to claim 2, Features: In step S1, the raw materials for preparing the strontium calcium sulfate precursor solution are the following components in parts by weight: 0.15-0.6 parts of strontium chloride, 0.9-1 parts of calcium chloride, and 1.4-1.8 parts of sodium sulfate.

4. A method for preparing a composite feed additive containing strontium and calcium sulfate according to any one of claims 1 to 3, Features: The specific steps include: ① Place strontium calcium sulfate in a beaker, add deionized water to disperse, add N-acetylcysteine ​​and mix well, raise the reaction temperature to 80-90°C, stir the reaction at 400-500rpm for 4-6h, centrifuge at 5000rpm for 20min, collect the precipitate, disperse it in a sodium hydroxide solution, maintain the reaction temperature at 30-35°C, and the reaction time is 30-40min. After the reaction system is cooled to room temperature, filter and collect the precipitate to obtain activated strontium calcium sulfate; ② Place carboxymethyl chitosan in deionized water, disperse and mix evenly with ultrasonic dispersion, add EDC and NHS, stir at 450-500 rpm for 4-5 hours at room temperature, add activated strontium calcium sulfate prepared in step ①, continue stirring for 10-12 hours, after the reaction is completed, centrifuge at 5000 rpm for 10 minutes, collect the precipitate, and dry in vacuum to obtain carboxymethyl chitosan modified strontium calcium sulfate; ③ Disperse hyaluronic acid in deionized water, add the carboxymethyl chitosan modified strontium calcium sulfate prepared in step ②, add EDC and NHS, stir and react at 500-550 rpm, centrifuge at 5000 rpm for 15 min after 20-24 h, collect the precipitate, and freeze-dry to obtain modified strontium calcium sulfate powder; ④ Mix the modified strontium calcium sulfate prepared in step ③ with deionized water and inject into a mold with mold parameters of 10 mm in diameter and 3 mm in height. After curing, a composite feed additive is obtained.

5. The method for preparing the composite feed additive containing strontium and calcium sulfate according to claim 4, Features: In step ①, the mass ratio of strontium calcium sulfate to N-acetylcysteine ​​is 4:1-2; the mass concentration of sodium hydroxide in the sodium hydroxide solution is 5-10 g / L, and the mass volume ratio of strontium calcium sulfate to sodium hydroxide solution is 0.06-0.08 g / mL.

6. The method for preparing the composite feed additive containing strontium and calcium sulfate according to claim 5, Features: In step ②, the mass ratio of the EDC to carboxymethyl chitosan is 2.5-3:1, and the mass ratio of the NHS to carboxymethyl chitosan is 1.5-2:

1.

7. The method for preparing the composite feed additive containing strontium and calcium sulfate according to claim 6, Features: In step ③, the mass ratio of EDC to hyaluronic acid is 4-5:1, and the mass ratio of NHS to hyaluronic acid is 2.5-3:

1.

8. The method for preparing the composite feed additive containing strontium and calcium sulfate according to claim 7, Features: In step ④, the mass volume ratio between the modified strontium calcium sulfate and deionized water is 1-1.5 g / mL.

Citation Information

Patent Citations

  • Calcium sulphate composite bone renovation material, preparation method and application thereof

    CN101269241A

  • Plant source disease-resistant growth-promoting feedstuff additive and preparation method thereof

    CN101341926A

  • Method for purifying strontium sulfate and co-producing calcium sulfate and industrial salt by using strontium sulfate waste residues

    CN102092763A

  • Biodegradable strontium-doped calcium sulfate material having biological activity, and its preparation method and use

    CN102430147A

  • Selenium strontium feed additive as well as production process and use method of selenium strontium feed additive

    CN102640859A