Vacuum cup made of heat-insulating material with low heat conductivity coefficient
By coating the heat-insulating coating of silica aerogel and glass microbead composite material on the inner and outer wall of the thermos cup, combined with polyaniline microcapsules, the problem of poor insulation effect of high-temperature substances in the prior art is solved, and the problem of poor insulation effect of high-temperature substances is achieved. Better insulation and long-term insulation performance.
Patent Information
- Application Number
- CN202410967565.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The existing thermos cups are not effective in the insulation of high-temperature substances, and the need cannot be met by relying solely on vacuum structure insulation.
The thermal insulation cup is used for low thermal conductivity insulation. By coating the thermal insulation coating on the inner and outer walls of the vessel, a composite material of silica aerogel and glass microbeads is used, and a polyaniline microcapsules are combined to improve the thermal insulation performance.
It significantly reduces the heat loss of the thermos cup, improves the insulation effect, and enhances the stability and long-term insulation performance of the thermal insulation coating.
Smart Images

Figure BDA0004952190160000081 
Figure BDA0004952190160000091
Abstract
Description
Technical Field
[0001] The present application relates to the field of thermos cups, and in particular to a thermos cup made of insulating material with low thermal conductivity. Background Art
[0002] Thermos cups usually have a lid on the top and are tightly sealed, which can delay the heat dissipation of water or other liquids inside to achieve the purpose of heat preservation.
[0003] In order to further improve the thermal insulation effect of the thermos cup, a shell is usually added to the outside of the thermos cup, and a vacuum structure is used for thermal insulation inside. As the quality requirements for thermos cups increase, the thermal insulation effect of thermos cups has also been improved. And it is not just for storing ordinary liquids, there is also a demand for thermal insulation of substances with higher temperatures. Using only vacuum structure insulation cannot meet the thermal insulation needs. Summary of the invention
[0004] In order to improve the heat preservation performance of a thermos cup, the present application provides a thermos cup made of an insulating material with a low thermal conductivity coefficient.
[0005] The low thermal conductivity insulation material thermos cup provided in this application adopts the following technical solution: A low thermal conductivity insulation material thermos cup, comprising a thermos cup liner and a thermos cup shell, wherein the thermos cup liner comprises an liner body and a thermal insulation coating, wherein the thermal insulation coating is obtained by coating the thermal insulation coating on the outer wall of the liner body, and the thermal insulation coating comprises the following components by mass: 48-52 parts of acrylic resin, 19-21 parts of glass microsphere composite material, 27-29 parts of silica aerogel; 2-4 parts of dispersant, 4-6 parts of deionized water.
[0006] By adopting the above technical scheme, a layer of thermal insulation coating is applied on the outer wall of the inner liner body, which can effectively reduce heat loss, thereby playing a role in heat preservation of the inner liner, thereby improving the thermal insulation effect of the thermos cup and reducing the heat loss of the thermos cup. A composite component of silica aerogel and glass microbeads is added to the thermal insulation coating. Both silica aerogel and glass microbeads have good thermal insulation properties. After the two are compounded, the thermal insulation properties of the coating can be further improved.
[0007] Preferably, the glass microsphere composite material comprises modified porous glass microspheres and polyaniline microcapsules.
[0008] By adopting the above technical scheme, after the porous glass microspheres are compounded with the polyaniline microcapsules, the polyaniline microcapsules are embedded in the pore structure of the glass microspheres, so that the prepared glass microsphere composite material is stably combined with the polyaniline microcapsules. The polyaniline microcapsules have good interface bonding properties, so that the glass microsphere composite material can be more fully combined in the resin system, thereby making the prepared thermal insulation coating more stable, further improving the thermal insulation performance of the inner liner body.
[0009] Preferably, the polyaniline microcapsules include a phase change microcapsule preform, aniline and nano zinc oxide.
[0010] By adopting the above technical scheme, multilayer phase change microcapsules are obtained by compounding phase change microcapsules preforms, aniline and nano zinc oxide, which have the advantages of large energy storage density and stable chemical properties, and have good thermal insulation performance, further reducing the occurrence of heat loss in the thermos cup, and the polyaniline microcapsules prepared with aniline as raw material make the prepared thermal insulation coating have good toughness, and can maintain good stability after the inner liner body is heated and expanded, further improving the long-term thermal insulation performance of the inner liner body.
[0011] Preferably, the polyaniline microcapsules are prepared by the following method: After mixing n-docosane, sodium dodecyl sulfate, tetrabutyl titanate and formamide, the mixture is stirred under oil bath conditions, then formamide is added, the mixture is reacted under oil bath stirring conditions, filtered and washed to obtain a phase change microcapsule preform; after mixing the phase change microcapsule preform, a surfactant and deionized water, the mixture is stirred under ice bath conditions, the pH value of the system is adjusted to 1.3-1.7, aniline and nano zinc oxide are added, the mixture is stirred, ammonium persulfate is added for reaction, filtered and washed, and polyaniline microcapsules are obtained after drying.
[0012] By adopting the above technical scheme, a phase change microcapsule preform is prepared with docosane as the core material and titanium dioxide as the first shell layer, and then a titanium source is added to make tetrabutyl titanate evenly distributed on the surface of the phase change microcapsule preform to form stable micelles, and then a surfactant is used to make the surface of the phase change microcapsule preform, and formamide is continued to be added to make tetrabutyl titanate hydrolyze to form titanium dioxide with a stable network structure. The obtained polyaniline microcapsule has a smooth surface and good stability, and can play a good thermal insulation performance, thereby improving the overall thermal insulation performance of the thermal insulation coating.
[0013] Preferably, the mass ratio of the phase change microcapsule preform, aniline and nano zinc oxide is 1:(0.2-0.4):0.07.
[0014] By adopting the above technical solution, the mass ratio of the phase change microcapsule preform, aniline and nano zinc oxide is preferably within the above range, which can further improve the overall stability of the prepared polyaniline microcapsules.
[0015] Preferably, the modified porous glass microspheres include hollow glass microspheres and a silane coupling agent.
[0016] Preferably, the modified porous glass microspheres are prepared by the following method: The hollow glass microspheres are mixed with a sodium hydroxide aqueous solution, stirred and then washed to obtain porous glass microspheres; the silane coupling agent is mixed with anhydrous ethanol, the pH value is adjusted to acidic, the porous glass microspheres are added and stirred, and the modified porous glass microspheres are washed and then dried to obtain the modified porous glass microspheres.
[0017] By adopting the above technical solution, the surface of the hollow glass microspheres is modified with a silane coupling agent, so that the bonding performance between the glass microspheres and the resin system is improved, so that the system has good mechanical properties, and the glass microspheres can be better dispersed in the coating, further improving the uniformity of the coating, thereby improving the thermal insulation performance of the inner liner body.
[0018] Preferably, the silane coupling agent is KH560.
[0019] Preferably, the mass ratio between the porous glass microbeads and the silane coupling agent is (12.5-13.5):1.
[0020] By adopting the above technical solution, preferably the mass ratio between the porous glass microbeads and the silane coupling agent is within the above range, the stability of the prepared modified porous glass microbeads can be further improved.
[0021] Preferably, the thermal insulation coating is prepared by the following method: The glass microbead composite material, silica aerogel, dispersant, acrylic resin and deionized water are mixed, heated and stirred to obtain a heat-insulating coating.
[0022] In summary, the present application includes at least one of the following beneficial technical effects: 1. A thermal insulation coating is applied to the inner liner of the thermos cup, so that a thermal insulation coating is formed on the outer wall of the inner liner. The thermal insulation coating contains a composite material of silica aerogel and glass microbeads. The combination of the two can effectively improve the overall thermal insulation performance of the thermal insulation coating, so that the prepared thermal insulation coating has good thermal insulation performance; 2. The glass microsphere composite material is obtained by embedding polyaniline microcapsules into the void structure of porous glass microspheres. The polyaniline microcapsules have good interface bonding properties, which can better bond the porous glass microspheres with the resin material, thereby making the glass microspheres more stable in the thermal insulation coating, thereby further improving the thermal insulation performance of the thermal insulation coating; 3. n-Docosane is used as a profile to be coated in the titanium dioxide shell of the microcapsule, so that n-Docosane can be released in the thermal insulation coating system to achieve long-term thermal insulation performance. In addition, n-Docosane has a self-regulating effect and can store energy to further improve the stability of the thermal insulation coating; 4. The porous glass microspheres are modified with dopamine and silane coupling agents. On the one hand, the interfacial bonding ability between the porous glass microspheres and the resin system is improved, so that the glass microsphere composite material can be better combined with the system. On the other hand, the polyaniline microcapsules can be more stable in the voids of the porous glass microspheres, thereby improving the overall performance of the thermal insulation coating. DETAILED DESCRIPTION
[0023] The present application is further described in detail below with reference to the embodiments: Description of raw materials: All raw materials in the examples are commercially available; wherein the coupling agent is KH560 (CAS No.: 2530-83-8); the surfactant is sodium dodecyl sulfate (CAS No.: 151-21-3); and the dispersant is polypropylene alcohol (CAS No.: 25791-96-2).
[0024] Example 1 Preparation of modified porous glass microspheres: The hollow glass microspheres were calcined at 400°C in a muffle furnace, added to a 0.1 mol / L sodium hydroxide aqueous solution, stirred at 190°C for 1.5 hours, cooled to 25°C while stirring, and then washed with deionized water to obtain porous glass microspheres; 1.11 g of a silane coupling agent was mixed with 15 g of anhydrous ethanol, the pH value was adjusted to 4 with acetic acid, 13.89 g of porous glass microspheres were added, stirred at 300 r / min for 2 hours, washed with deionized water, and dried in a vacuum drying oven at 50°C for 12 hours to obtain modified porous glass microspheres.
[0025] Preparation of polyaniline microcapsules: 23.15 g of n-docosane (CAS No.: 629-97-0), 3.7 g of sodium dodecyl sulfate (CAS No.: 151-21-3), 23.15 g of tetrabutyl titanate (CAS No.: 5593-70-4) and 350 g of formamide (CAS No.: 75-12-7) were mixed, and stirred at 500 r / min for 5 h in an oil bath at 50 ° C to emulsify the system, and then 40 g of formamide was added, and the reaction was continued for 4 h under stirring in the oil bath. After filtering, the mixture was washed alternately with deionized water and anhydrous ethanol. The mixture was washed 3 times to obtain a phase change microcapsule preform; 39.37 g of the phase change microcapsule preform prepared above, 6 g of a surfactant, and 20 g of deionized water were mixed, and the mixture was stirred at a speed of 600 r / min for 30 min in an ice bath, and the pH value of the system was adjusted to 1.3 with hydrochloric acid, 7.87 g of aniline (CAS No.: 62-53-3) and 2.76 g of nano zinc oxide were added, and the stirring was maintained for 1 h, 50 g of ammonium persulfate was added, and the mixture was allowed to stand for reaction and then filtered. After washing with deionized water, the mixture was dried at a temperature of 30° C. to obtain polyaniline microcapsules.
[0026] Preparation of glass microsphere composite components: 9.78 g of porous glass microbeads, 41.09 g of polyaniline microcapsules and 39.13 g of acetone were mixed and ultrasonically dispersed for 10 min. The mixture was allowed to stand at 25 °C for 12 h, and then transferred to an oven at 50 °C for 6 h. The mixture was then filtered, washed with deionized water, and dried in an oven at 50 °C to remove the acetone to obtain a glass microbead composite component.
[0027] Preparation of silica aerogel: Tetraethoxysilane, anhydrous ethanol, deionized water and hydrochloric acid were mixed in a molar ratio of 1:4:1.85:2×10 -6 The mixture was mixed, condensed and refluxed for 8 hours to obtain a silica ethanol solution. After mixing n-hexane and the silica ethanol solution in a mass ratio of 3:7, ammonia was added, and after standing for 5 minutes, the mixture was transferred to 80°C and maintained for 2 hours. Then, the mixture was dried at 180°C for 2 hours and crushed to obtain silica aerogel.
[0028] Preparation of thermal insulation coating: 19 g of glass microsphere composite material, 27 g of silica aerogel, 2 g of dispersant, 48 g of acrylic resin and 4 g of deionized water were mixed, the temperature was raised to 70° C., and the mixture was stirred at a speed of 900 r / min for 40 min to obtain a thermal insulation coating.
[0029] Prepare the thermos cup: The heat-insulating coating is coated on the outer wall of the inner liner body, so that a layer of heat-insulating coating is formed on the outer wall of the inner liner body and a thermos cup inner liner is obtained. The thermos cup inner liner is assembled with the thermos cup outer shell to obtain the thermos cup.
[0030] Example 2 Preparation of modified porous glass microspheres: The hollow glass microspheres were calcined at 400°C in a muffle furnace, added to a 0.1 mol / L sodium hydroxide aqueous solution, stirred at 190°C for 1.5 hours, cooled to 25°C while stirring, and then washed with deionized water to obtain porous glass microspheres; 1.03 g of a silane coupling agent was mixed with 15 g of anhydrous ethanol, the pH value was adjusted to 4 with acetic acid, 13.97 g of porous glass microspheres were added, stirred at a speed of 300 r / min for 2 hours, washed with deionized water, and dried in a vacuum drying oven at 50°C for 12 hours to obtain modified porous glass microspheres.
[0031] Preparation of polyaniline microcapsules: 23.15g of n-docosane, 3.7g of sodium dodecyl sulfate, 23.15g of tetrabutyl titanate and 350g of formamide were mixed, and stirred at a speed of 500r / min for 5h in an oil bath at 50°C to emulsify the system, and then 40g of formamide was added, and the reaction was continued for 4h under stirring in the oil bath. After filtering, deionized and anhydrous ethanol were used to wash alternately 3 times to obtain a phase change microcapsule preform; 34.01g of the phase change microcapsule preform prepared above, 6g of a surfactant, and 20g of deionized water were mixed, and stirred at a speed of 600r / min for 30min under ice bath conditions, and the pH value of the system was adjusted to 1.7 with hydrochloric acid, 13.61g of aniline and 2.38g of nano zinc oxide were added, and stirring was maintained for 1h, and 50g of ammonium persulfate was added. After standing for reaction, it was filtered, washed with deionized water, and dried at a temperature of 30°C to obtain polyaniline microcapsules.
[0032] Preparation of glass microsphere composite components: 9.78 g of porous glass microbeads, 41.09 g of polyaniline microcapsules and 39.13 g of acetone were mixed and ultrasonically dispersed for 10 min. The mixture was allowed to stand at 25 °C for 12 h, and then transferred to an oven at 50 °C for 6 h. The mixture was then filtered, washed with deionized water, and dried in an oven at 50 °C to remove the acetone to obtain a glass microbead composite component.
[0033] Preparation of silica aerogel: Tetraethoxysilane, anhydrous ethanol, deionized water and hydrochloric acid were mixed in a molar ratio of 1:4:1.85:2×10 -6The mixture was mixed, condensed and refluxed for 8 hours to obtain a silica ethanol solution. After mixing n-hexane and the silica ethanol solution in a mass ratio of 3:7, ammonia was added, and after standing for 5 minutes, the mixture was transferred to 80°C and maintained for 2 hours. Then, the mixture was dried at 180°C for 2 hours and crushed to obtain silica aerogel.
[0034] Preparation of thermal insulation coating: 21 g of glass microsphere composite material, 29 g of silica aerogel, 4 g of dispersant, 52 g of acrylic resin and 6 g of deionized water were mixed, the temperature was raised to 70° C., and the mixture was stirred at a speed of 900 r / min for 40 min to obtain a thermal insulation coating.
[0035] Prepare the thermos cup: The heat-insulating coating is coated on the outer wall of the inner liner body, so that a layer of heat-insulating coating is formed on the outer wall of the inner liner body and a thermos cup inner liner is obtained. The thermos cup inner liner is assembled with the thermos cup outer shell to obtain the thermos cup.
[0036] Example 3 Preparation of modified porous glass microspheres: The hollow glass microspheres were calcined at 400°C in a muffle furnace, added to a 0.1 mol / L sodium hydroxide aqueous solution, stirred at 190°C for 1.5 hours, cooled to 25°C while stirring, and then washed with deionized water to obtain porous glass microspheres; 1.07 g of a silane coupling agent was mixed with 15 g of anhydrous ethanol, the pH value was adjusted to 4 with acetic acid, 13.93 g of porous glass microspheres were added, stirred at a speed of 300 r / min for 2 hours, washed with deionized water, and dried in a vacuum drying oven at 50°C for 12 hours to obtain modified porous glass microspheres.
[0037] Preparation of polyaniline microcapsules: 23.15 g of n-docosane, 3.7 g of sodium dodecyl sulfate, 23.15 g of tetrabutyl titanate and 350 g of formamide were mixed, and stirred at 500 r / min for 5 h in an oil bath at 50° C. to emulsify the system, and then 40 g of formamide was added, and the mixture was continued to react for 4 h in an oil bath with stirring. After filtering, the mixture was washed alternately with deionized and anhydrous ethanol for 3 times to obtain a phase change microcapsule preform; 36.5 g of the phase change microcapsule preform prepared above, 6 g of a surfactant and 20 g of deionized water were mixed, and the mixture was stirred at 600 r / min for 30 min in an ice bath, and the pH value of the system was adjusted to 1.5 with hydrochloric acid, 10.95 g of aniline and 2.55 g of nano zinc oxide were added, and stirring was maintained for 1 h, 50 g of ammonium persulfate was added, and the mixture was filtered after standing for reaction, washed with deionized water, and dried at 30° C. to obtain polyaniline microcapsules.
[0038] Preparation of glass microsphere composite components: 9.78 g of porous glass microbeads, 41.09 g of polyaniline microcapsules and 39.13 g of acetone were mixed and ultrasonically dispersed for 10 min. The mixture was allowed to stand at 25 °C for 12 h, and then transferred to an oven at 50 °C for 6 h. The mixture was then filtered, washed with deionized water, and dried in an oven at 50 °C to remove the acetone to obtain a glass microbead composite component.
[0039] Preparation of silica aerogel: Tetraethoxysilane, anhydrous ethanol, deionized water and hydrochloric acid were mixed in a molar ratio of 1:4:1.85:2×10 -6 The mixture was mixed, condensed and refluxed for 8 hours to obtain a silica ethanol solution. After mixing n-hexane and the silica ethanol solution in a mass ratio of 3:7, ammonia was added, and after standing for 5 minutes, the mixture was transferred to 80°C and maintained for 2 hours. Then, the mixture was dried at 180°C for 2 hours and crushed to obtain silica aerogel.
[0040] Preparation of thermal insulation coating: 20 g of glass microsphere composite material, 28 g of silica aerogel, 3 g of dispersant, 50 g of acrylic resin and 5 g of deionized water were mixed, the temperature was raised to 70° C., and the mixture was stirred at a speed of 900 r / min for 40 min to obtain a thermal insulation coating.
[0041] Prepare the thermos cup: The heat-insulating coating is coated on the outer wall of the inner liner body, so that a layer of heat-insulating coating is formed on the outer wall of the inner liner body and a thermos cup inner liner is obtained. The thermos cup inner liner is assembled with the thermos cup outer shell to obtain the thermos cup.
[0042] Example 4 Example 4 is based on Example 3. The difference between Example 4 and Example 3 is that in Example 4, when preparing the modified porous glass microspheres, 1.25 g of silane coupling agent and 13.75 g of porous glass microspheres are used.
[0043] Example 5 Example 5 is based on Example 3. The difference between Example 5 and Example 3 is that in Example 5, when preparing porous glass microbeads, 0.94 g of silane coupling agent and 14.06 g of porous glass microbeads are used.
[0044] Example 6 Example 6 is based on Example 3. The difference between Example 6 and Example 3 is that in Example 6, the silane coupling agent used in preparing the porous glass microbeads is KH550 (CAS No.: 919-30-2).
[0045] Example 7 Example 7 is based on Example 3. The difference between Example 7 and Example 3 is that the porous microbeads are not modified in Example 7.
[0046] Example 8 Example 8 is based on Example 3. The difference between Example 8 and Example 3 is that in Example 8, 42.74 g of phase change microcapsule preform, 4.27 g of aniline and 2.99 g of nano zinc oxide are used in preparing polyaniline microcapsules.
[0047] Example 9 Example 9 is based on Example 3. The difference between Example 9 and Example 3 is that when preparing polyaniline microcapsules in Example 9, 29.94 g of phase change microcapsule preform, 17.96 g of aniline and 2.1 g of nano zinc oxide are used.
[0048] Example 10 Example 10 is based on Example 3. The difference between Example 10 and Example 3 is that when preparing polyaniline microcapsules in Example 10, the pH value is 1.
[0049] Embodiment 11 Example 11 is based on Example 3. The difference between Example 11 and Example 3 is that when preparing polyaniline microcapsules in Example 11, the pH value is 2.
[0050] Example 12 Example 12 is based on Example 3. The difference between Example 12 and Example 3 is that in Example 12, no nano zinc oxide is added when preparing polyaniline microcapsules.
[0051] Embodiment 13 Example 13 is based on Example 3. The difference between Example 13 and Example 3 is that when preparing the thermal insulation coating in Example 13, the glass microbead composite component added is xg and the acrylic resin added is xg.
[0052] Embodiment 14 Example 14 is based on Example 3. The difference between Example 14 and Example 3 is that when preparing the thermal insulation coating in Example 14, the glass microbead composite component added is xg and the acrylic resin added is xg.
[0053] Comparative Example 1 Comparative Example 1 is based on Example 3. When preparing the glass microsphere composite component, Comparative Example 1 only mixes the glass microspheres and polyaniline capsules in a normal manner.
[0054] Comparative Example 2 Comparative Example 2 is based on Example 3, and in Comparative Example 2, the porous glass microspheres are replaced with ordinary glass microspheres.
[0055] Comparative Example 3 Comparative Example 3 is based on Example 3, and the glass microsphere composite material in Comparative Example 3 is replaced by polyaniline microcapsules.
[0056] Performance testing The samples of Examples 1-14 and Comparative Examples 1-2 were sampled and the following performance tests were performed: (1) Thermal insulation performance test The thermal insulation performance of the thermal insulation coating of each sample was tested. Each sample was tested three times, the average value was taken, and the test results were filled in Table 1.
[0057] (2) Thermal aging performance test The ambient humidity was controlled at 95% RH, and the samples were subjected to wet heat aging at a cyclic temperature of 150-200°C for 24 hours. The thermal insulation performance of the samples was retested. Each sample was tested three times, and the average value was taken. The test results were filled in Table 1.
[0058] (3) Toughness test The tensile strength of the thermal insulation coating of each sample was tested three times, and the average value was taken. The test results were filled in Table 1.
[0059] Table 1 Performance test results of Examples 1-14 and Comparative Examples 1-2 Data analysis The thermal conductivity coefficients of Examples 1-3 are all 0.09 W / m·k or below, indicating that the thermal insulation coating prepared in the present application has good thermal insulation performance. The thermal aging performance of Examples 1-3 is all 0.12 W / m·k or below, indicating that the thermal insulation coating prepared in the present application has a long-term thermal insulation effect. The tensile strength of Examples 1-3 is all 49 MPa or above, indicating that the thermal insulation coating prepared in the present application has good tensile resistance.
[0060] In Example 4 and Example 5, when preparing modified porous glass microspheres, the mass ratio of the silane coupling agent to the porous glass microspheres is not within the range specified in the present application. When the content of the silane coupling agent is too little, the improvement effect on the surface of the hollow glass microspheres is difficult to be improved, resulting in a decrease in the binding performance of the glass microspheres in the resin system and a decrease in uniformity, thereby affecting the overall stability of the system. When the content of the silane coupling agent is too much, the stability of the system will also decrease, affecting the comprehensive performance of the system.
[0061] In Example 6, the silane coupling agent KH560 was replaced by KH550. Although there was some improvement on the overall system, it was slightly worse than the improvement effect of using KH560 on porous glass microspheres.
[0062] In Example 7, the porous glass microbeads were not modified using a silane coupling agent. The interface bonding ability between the unmodified porous glass microbeads and the resin system was weak, and the stability of the void structure of the polyaniline microcapsules loaded in the porous glass microbeads was also reduced.
[0063] In Example 8 and Example 9, when preparing polyaniline microcapsules, the mass ratios of the phase change microcapsule preform, aniline and nano-zinc oxide are not within the range specified in the present application. When the aniline content is too low, the obtained polyaniline is too low, the binding performance with the nano-zinc oxide particles is reduced, the chemical activity is reduced, and the stability of the prepared polyaniline microcapsules is reduced, which affects the thermal insulation performance of the polyaniline microcapsules. When the aniline content is too high, the particle size of the prepared polyaniline microcapsules is too large, the particle size uniformity of the polyaniline microcapsules is reduced, and the stability of the system is reduced.
[0064] When preparing polyaniline microcapsules, a pH value that is too high or too low in the system is not conducive to the oxidative polymerization process of polyaniline, which reduces the stability of the system. Therefore, the comprehensive performance of Example 10 and Example 11 is reduced.
[0065] In Example 12, nano zinc oxide is not added. The absence of nano zinc oxide will affect the chemical activity of polyaniline during bonding, thereby reducing the stability of the prepared polyaniline.
[0066] In Example 13 and Example 14, when preparing the thermal insulation coating, the addition amount of the glass microbead composite component is changed. When the content of the glass microbead composite component is too little, the problem of improving the thermal insulation effect of the thermal insulation coating system is further increased. When the content of the glass microbead composite component is too much, the glass microbead composite component is difficult to be evenly distributed in the system, making it difficult for the glass microbead composite component to be evenly arranged, which affects the overall thermal insulation performance of the system and affects the mechanical properties of the prepared thermal insulation coating.
[0067] In Comparative Example 1, the modified porous glass microspheres were replaced with hollow glass microspheres, and the polyaniline microcapsules were difficult to load and were free in the system, with reduced stability, which affected the thermal insulation performance of the prepared thermal insulation coating.
[0068] In Comparative Example 2, the glass microsphere composite material is only modified glass microspheres, and the system without adding polyaniline microcapsules is difficult to further improve the overall thermal insulation performance of the thermal insulation coating.
[0069] In Comparative Example 3, the glass microsphere composite material is replaced with polyaniline microcapsules. On the one hand, the polyaniline microcapsules are difficult to load and are free in the system, and the stability is difficult to decrease. On the other hand, without the hollow structure of the hollow glass microspheres with stable arrangement, the overall thermal insulation performance and mechanical properties of the thermal insulation coating are affected.
[0070] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A low thermal conductivity insulation material thermos cup, characterized by: The invention comprises a thermos cup liner and a thermos cup shell, wherein the thermos cup liner comprises an inner liner body and a heat-insulating coating, wherein the heat-insulating coating is obtained by coating the heat-insulating coating on the outer wall of the inner liner body, and the heat-insulating coating comprises the following components by mass: 48-52 parts of acrylic resin, 19-21 parts of glass microsphere composite material, 27-29 parts of silica aerogel; 2-4 parts of dispersant, 4-6 parts of deionized water.
2. A low thermal conductivity insulation material thermos cup according to claim 1, characterized in that: The glass microsphere composite material comprises modified porous glass microspheres and polyaniline microcapsules.
3. A low thermal conductivity insulation material thermos cup according to claim 2, characterized in that: The polyaniline microcapsule comprises a phase-change microcapsule preform, aniline and nano zinc oxide.
4. A low thermal conductivity insulation material thermos cup according to claim 2, characterized in that: The polyaniline microcapsules are prepared by the following method: After mixing n-docosane, sodium dodecyl sulfate, tetrabutyl titanate and formamide, the mixture is stirred under oil bath conditions, then formamide is added, the mixture is reacted under oil bath stirring conditions, filtered and washed to obtain a phase change microcapsule preform; after mixing the phase change microcapsule preform, a surfactant and deionized water, the mixture is stirred under ice bath conditions, the pH value of the system is adjusted to 1.3-1.7, aniline and nano zinc oxide are added, the mixture is stirred, ammonium persulfate is added for reaction, filtered and washed, and polyaniline microcapsules are obtained after drying.
5. A low thermal conductivity insulation material thermos cup according to claim 4, characterized in that: The mass ratio of the phase change microcapsule preform, aniline and nano zinc oxide is 1:(0.2-0.4):0.
07.
6. The low thermal conductivity insulation material thermos cup according to claim 1, characterized in that: The modified porous glass microspheres include hollow glass microspheres and a silane coupling agent.
7. A low thermal conductivity insulation material thermos cup according to claim 6, characterized in that: The modified porous glass microspheres are prepared by the following method: The hollow glass microspheres are mixed with a sodium hydroxide aqueous solution, stirred and then washed to obtain porous glass microspheres; the silane coupling agent is mixed with anhydrous ethanol, the pH value is adjusted to acidic, the porous glass microspheres are added and stirred, and the modified porous glass microspheres are washed and then dried to obtain the modified porous glass microspheres.
8. The low thermal conductivity insulation material thermos cup according to claim 6, characterized in that: The silane coupling agent is KH560.
9. The low thermal conductivity insulation material thermos cup according to claim 6, characterized in that: The mass ratio between the porous glass microbeads and the silane coupling agent is (12.5-13.5):
1.
10. The low thermal conductivity insulation material thermos cup according to claim 1, characterized in that: The thermal insulation coating is prepared by the following method: glass microbead composite material, silicon dioxide aerogel, dispersant, acrylic resin and deionized water are mixed, heated and stirred to obtain the thermal insulation coating.