Hydrogel with photo-thermal antibacterial property and preparation method thereof

By loading lipid nanoparticles with specific compounds in the hydrogel, combined with protein and polysaccharide cross-linking technology, a hydrogel with photothermal antibacterial properties was prepared, which solved the problem of carrying stability of active ingredients in cosmetics and improved the cosmetics' Functionality and application potential.

CN118902876AInactive Publication Date: 2024-11-08BEIJING TECH & BUSINESS UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410972532.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively and stably carry active ingredients in cosmetics, and the application of photothermal hydrogels in medical and industrial fields has not been fully combined and has not met the diverse needs of cosmetics.

Method used

A hydrogel matrix formed by crosslinking protein substances and polysaccharide substances, and loading lipid nanoparticles wrapped with specific compounds on it to form a hydrogel with photothermal antibacterial properties. Through calcium salt crosslinking technology preparation.

Benefits of technology

The excellent light response and heat conversion ability of the hydrogel is achieved, which significantly improves the treatment and healing effect of wound infection, and at the same time shows good moisturizing and antibacterial properties in cosmetics, with huge development potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118902876A_ABST
    Figure CN118902876A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hydrogel, and particularly relates to hydrogel with photo-thermal antibacterial property and a preparation method thereof, the hydrogel with photo-thermal antibacterial property comprises a hydrogel matrix and lipid nanoparticles loaded on the hydrogel; a compound as shown in a formula (I) is wrapped in the lipid nanoparticles. Compared with the prior art, the compound as shown in the hydrophobic molecular formula (I) is prepared into the nano-particles, the nano-particles are combined with the hydrogel matrix, the hydrogel with the photo-thermal antibacterial characteristic is obtained, and the hydrogel has excellent photo-response and thermal conversion capacity, has remarkable advantages in the aspects of treating wound infection and promoting wound healing, and has good application prospects. And huge development potential is shown in the aspects of biological medicines, cosmetics and the like. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogels, and in particular relates to a hydrogel with photothermal antibacterial properties and a preparation method thereof. Background Art

[0002] Hydrogel is a type of polymer with a three-dimensional network structure that has hydrophilic groups and can be swollen by water but is insoluble in water. It can absorb a large amount of water in water and swell significantly, and after swelling significantly, it can continue to maintain its original structure without being dissolved.

[0003] The photothermal effect of hydrogel is a new technology applied in medical and industrial fields. Its principle is to utilize the absorption and conversion of light by hydrogel materials to convert light energy into heat energy, thereby producing a corresponding thermal effect. In recent years, the excellent light response and thermal conversion capabilities of photothermal hydrogel have made it the focus of attention. It has significant advantages in treating wound infections and promoting wound healing, and has great potential for development in biomedicine, cosmetics and other fields.

[0004] Cosmetics is a general term for products used for the purpose of makeup, and has increasingly become a necessity in human life. In recent years, people's demand for cosmetics has also increased, and the requirements for cosmetics have also increased. The status of functional cosmetics in the cosmetics market has received more attention, and how to stably and efficiently deliver active ingredients has become the main issue in the research of such cosmetics. The combination of photothermal water gel and cosmetics is a new development direction, which can give cosmetics the excellent properties of photothermal water gel to meet people's needs. Therefore, it is of great significance to develop an effective combination of photothermal water gel and cosmetics. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a hydrogel with photothermal antibacterial properties and a preparation method thereof.

[0006] The present invention provides a hydrogel with photothermal antibacterial properties, comprising a hydrogel matrix and lipid nanoparticles loaded on the hydrogel; the lipid nanoparticles contain a compound represented by formula (I);

[0007]

[0008] Preferably, the hydrogel matrix is ​​formed by cross-linking protein substances and polysaccharide substances; the mass ratio of the protein substances to the polysaccharide substances is 1:(0.1-1).

[0009] Preferably, the protein substance is selected from gelatin and / or silk fibroin; the polysaccharide substance is selected from one or more of alginate, hyaluronic acid and chitosan.

[0010] Preferably, the lipid nanoparticles comprise phospholipid polyethylene glycol and / or phospholipid polyethylene glycol derivatives.

[0011] Preferably, the mass ratio of the hydrogel matrix to the lipid nanoparticles is 1:(0.00001-0.0005).

[0012] The present invention also provides a method for preparing a hydrogel having photothermal antibacterial properties, comprising the following steps:

[0013] The protein substance is dissolved in an aqueous solution, and then a polysaccharide substance is added and dissolved, and then lipid nanoparticles are added and mixed continuously, and the mixture is allowed to stand at low temperature, and cross-linked with a calcium salt solution to obtain a hydrogel having photothermal antibacterial properties; the lipid nanoparticles contain a compound represented by formula (I);

[0014]

[0015] Preferably, the compound represented by formula (I) is prepared according to the following method:

[0016] S1) reacting N,N-dimethylformamide with phosphorus oxychloride at low temperature, then adding the compound represented by formula (II) for reflux reaction to obtain the compound represented by formula (III);

[0017] S2) reacting the compound represented by formula (III) with the compound represented by formula (IV) in a protective atmosphere to obtain the compound represented by formula (I);

[0018]

[0019] Preferably, the lipid nanoparticles are prepared according to the following method:

[0020] Mixing an organic solution containing a compound represented by formula (I) and an organic solution containing a phospholipid compound to obtain a mixed solution;

[0021] The mixed solution was added into water and sonicated to obtain lipid nanoparticles.

[0022] The invention also provides a cosmetic comprising the hydrogel with photothermal antibacterial properties.

[0023] The present invention also provides the use of the compound represented by formula (I) in preparing a hydrogel having photothermal antibacterial properties;

[0024]

[0025] The present invention provides a hydrogel with photothermal antibacterial properties, comprising a hydrogel matrix and lipid nanoparticles loaded on the hydrogel; the lipid nanoparticles contain a compound represented by formula (I). Compared with the prior art, the present invention prepares the compound represented by hydrophobic molecular formula (I) into nanoparticles and combines them with the hydrogel matrix to obtain a hydrogel with photothermal antibacterial properties, and the hydrogel has excellent light response and thermal conversion capabilities, has significant advantages in treating wound infections and promoting wound healing, and also shows great development potential in biomedicine and cosmetics. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is the mass spectrum of compound 3 obtained in Example 1 of the present invention;

[0027] Figure 2 is a transmission electron microscopy image of the lipid nanoparticles obtained in Example 2 of the present invention;

[0028] Figure 3 This is a trend diagram of the BTP-Th NPs photothermal material obtained in Example 2 of the present invention when the light intensity is changed at a fixed concentration, and when the concentration is changed at a fixed light intensity;

[0029] Figure 4 This is a photothermal stability test diagram of the BTP-Th NPs photothermal material obtained in Example 2 of the present invention;

[0030] Figure 5 This is a photothermal conversion diagram of the BTP-Th NPs photothermal material obtained in Example 2 of the present invention;

[0031] Figure 6 The antibacterial rate and plate graph of the BTP-Th NPs photothermal material obtained in Example 2 of the present invention against Escherichia coli;

[0032] Figure 7 This is a diagram of the hemolysis experiment of the BTP-Th NPs photothermal material obtained in Example 2 of the present invention;

[0033] Figure 8 The hydrogel obtained in Example 3 of the present invention is at 500mW / cm 2 and 800mW / cm 2 Photothermal variation diagram below;

[0034] Fig. 9 This is a bar graph showing the average values ​​of skin water content of volunteers every 15 minutes;

[0035] Fig.10 This is a curve diagram of the change in water loss rate of the hydrogel over time in Example 3 of the present invention;

[0036] Fig.11This is a graph showing the test results of the hemolysis rate of the hydrogel in Example 3 of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] The present invention provides an application of a compound represented by formula (I) in preparing a hydrogel having photothermal antibacterial properties;

[0039]

[0040] The present invention provides a hydrogel with photothermal antibacterial properties, comprising a hydrogel matrix and lipid nanoparticles loaded on the hydrogel; the lipid nanoparticles contain a compound represented by formula (I);

[0041]

[0042] According to the present invention, the hydrogel matrix is ​​formed by cross-linking protein substances and polysaccharides; the mass ratio of the protein substances to the polysaccharides is preferably 1: (0.1-1), more preferably 1: (0.3-0.8), more preferably 1: (0.4-0.6), and most preferably 1: 0.5; the protein substances can be natural proteins that can form hydrogels that are well known to those skilled in the art, without any special restrictions, and are preferably gelatin and / or silk fibroin in the present invention; the polysaccharides can be natural polysaccharides that can form hydrogels that are well known to those skilled in the art, without any special restrictions, and are preferably one or more of alginate, hyaluronic acid and chitosan in the present invention, more preferably alginate, and more preferably sodium alginate.

[0043] The hydrogel matrix is ​​loaded with lipid nanoparticles; the mass ratio of the hydrogel matrix to the lipid nanoparticles is preferably 1:(0.00001-0.0005), more preferably 1:(0.00001-0.0002), and more preferably 1:(0.00005-0.00017); the lipid nanoparticles are encapsulated with the compound represented by formula (I); the mass concentration of the compound represented by formula (I) in the lipid nanoparticles is preferably 5%-15%, more preferably 6%-12%, more preferably 8%-11%, and most preferably 9%-10%; the lipid nanoparticles preferably include phospholipid polyethylene glycol and / or phospholipid polyethylene glycol derivatives, and in the embodiments provided by the present invention, DSPE-PEG is specifically used. 2000 Take this as an example to illustrate.

[0044] The present invention prepares the compound represented by the hydrophobic molecular formula (I) into nanoparticles and combines them with a hydrogel matrix to obtain a hydrogel with photothermal antibacterial properties. The hydrogel has excellent light response and thermal conversion capabilities, has significant advantages in treating wound infections and promoting wound healing, and also shows great development potential in biomedicine and cosmetics.

[0045] The present invention also provides a method for preparing the above-mentioned hydrogel with photothermal antibacterial properties, comprising the following steps: dissolving a protein substance in an aqueous solution, then adding a polysaccharide substance to dissolve, adding lipid nanoparticles and continuing to mix, standing at low temperature, and cross-linking with a calcium salt solution to obtain a hydrogel with photothermal antibacterial properties; the lipid nanoparticles contain a compound represented by formula (I);

[0046]

[0047] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.

[0048] According to the present invention, the compound represented by formula (I) is prepared according to the following method: S1) reacting N,N-dimethylformamide with phosphorus oxychloride under low temperature conditions, and then adding the compound represented by formula (II) for reflux reaction to obtain the compound represented by formula (III); S2) reacting the compound represented by formula (III) with the compound represented by formula (IV) in a protective atmosphere to obtain the compound represented by formula (I);

[0049]

[0050]

[0051] N,N-dimethylformamide and phosphorus oxychloride are reacted under low temperature conditions; in the present invention, it is preferred to first cool N,N-dimethylformamide to low temperature conditions and then add phosphorus oxychloride; the temperature of the low temperature conditions is preferably 0°C to 5°C; the phosphorus oxychloride is preferably added in a protective atmosphere; the protective atmosphere can be a protective atmosphere well known to those skilled in the art and is not particularly limited, and argon is preferably used in the present invention; the volume ratio of N,N-dimethylformamide to phosphorus oxychloride is preferably (3-8):1, more preferably (4-6):1, and more preferably 5:1; the reaction time is preferably 1-3h, more preferably 1.5-2.5h, and more preferably 2h.

[0052] After the reaction, the compound represented by formula (II) is added for reflux reaction; the ratio of the phosphorus oxychloride to the compound represented by formula (II) is preferably (1-5) mL: (200-500) mg, more preferably (1-4) mL: (250-450) mg, more preferably (1-3) mL: (300-400) mg, more preferably 2 mL: (350-400) mg, most preferably 2 mL: 380 mg; the compound represented by formula (II) is preferably dissolved in dichloroethane and added in the form of a solution; the mass concentration of the compound represented by formula (II) in the solution is preferably 15-25 mg / mL, more preferably 16-22 mg / mL, more preferably 18-20 mg / mL, and most preferably 19 mg / mL; the reflux reaction time is preferably 6-14 h, more preferably 8-12 h.

[0053] After the reflux reaction, it is preferably cooled to room temperature, water is added to quench the reaction, and then extracted with an organic solvent, washed, dried, and purified to obtain a compound represented by formula (III); the organic solvent is an organic solvent well known to those skilled in the art, and there is no special limitation. In the present invention, dichloromethane is preferably used; the washing is preferably carried out with water; the drying is preferably carried out with an inorganic desiccant, more preferably anhydrous sodium sulfate; the purification is preferably carried out with column chromatography; the eluent for the column chromatography is preferably petroleum ether and dichloromethane; the volume ratio of petroleum ether to dichloromethane is preferably 15:1.

[0054] In a protective atmosphere, the compound represented by formula (III) is reacted with the compound represented by formula (IV); the protective atmosphere can be any protective atmosphere well known to those skilled in the art, without any special restrictions, and preferably argon in the present invention; the mass ratio of the compound represented by formula (III) to the compound represented by formula (IV) is preferably 1: (0.5-2), more preferably 1: (0.5-1.5), and even more preferably 1: 1; the reaction is preferably carried out in an organic solvent; the organic solvent can be any organic solvent well known to those skilled in the art, without any special restrictions, and preferably in the present invention Chloroform and pyridine; the volume ratio of chloroform to pyridine is preferably 20:(0.1-1), more preferably 20:(0.3-0.8), more preferably 20:(0.4-0.6), and most preferably 20:0.5; in the present invention, it is preferred to first add chloroform and stir to dissolve, and then add pyridine; the stirring and dissolving time is preferably 3-8 min, more preferably 4-6 min, and more preferably 5 min; the reaction temperature is preferably 60°C-70°C, more preferably 65°C; the reaction time is preferably 15-30 h, more preferably 20-26 h, and more preferably 24 h.

[0055] After the reaction is completed, it is preferably cooled, and then most of the solvent is evaporated and removed, and the crude product is washed with methanol to remove excess compound represented by formula (IV), and then purified by column chromatography to obtain the compound represented by formula (I); the eluent for the column chromatography is preferably petroleum ether and dichloromethane; the volume ratio of petroleum ether to dichloromethane is preferably 1:1.

[0056] According to the present invention, the lipid nanoparticles are preferably prepared according to the following method: an organic solution containing the compound represented by formula (I) is mixed with an organic solution containing a phospholipid compound to obtain a mixed solution; the mixed solution is added to water and ultrasonicated to obtain lipid nanoparticles.

[0057] In a specific embodiment provided by the present invention, the concentration of the compound represented by formula (I) in the organic solution containing the compound represented by formula (I) is preferably 0.5 to 2 mg / mL, more preferably 0.5 to 1.5 mg / mL, further preferably 0.8 to 1.2 mg / mL, and most preferably 1 mg / mL; the solvent of the organic solution containing the compound represented by formula (I) is preferably tetrahydrofuran.

[0058] In a specific embodiment provided by the present invention, the concentration of the phospholipid compound in the organic solution containing the phospholipid compound is preferably 10 to 20 mg / mL, more preferably 12 to 18 mg / mL, more preferably 14 to 18 mg / mL, and most preferably 16 mg / mL; the phospholipid compound is preferably phospholipid polyethylene glycol and / or a phospholipid polyethylene glycol derivative, and in the embodiments provided by the present invention, DSPE-PEG is specifically used. 2000 Take this as an example to illustrate; the solvent in the organic solution containing phospholipid compounds is preferably tetrahydrofuran.

[0059] An organic solution in which a compound represented by formula (I) is dissolved is mixed with an organic solution containing a phospholipid compound; the mass of the compound represented by formula (I) is preferably 5% to 15% of the total mass of the compound represented by formula (I) and the phospholipid compound, more preferably 6% to 12%, further preferably 8% to 11%, and most preferably 9% to 10%.

[0060] The mixed solution is added to water and ultrasonicated to obtain lipid nanoparticles; the volume ratio of the mixed solution to water is preferably (0.2-1):10, more preferably (0.2-0.8):10, more preferably (0.4-0.6):10, more preferably (0.4-0.5):10, and most preferably (0.4875-0.5):10; the power of the ultrasound is preferably 100-500W; the time of the ultrasound is preferably 1-3h, more preferably 1.5-2.5h, and more preferably 2h; after the ultrasound, the tetrahydrofuran and excess water are preferably removed by heating to obtain lipid nanoparticles.

[0061] Dissolve the protein substance in the aqueous solution; the protein substance is the same as described above and will not be repeated here; the aqueous solution is preferably a buffer solution, more preferably a PBS buffer solution; the ratio of the protein substance to the aqueous solution is preferably 0.1g:(2-4)mL, more preferably 0.1g:(2-3)mL, and more preferably 0.1g:2.5mL; the dissolution temperature is preferably 37°C; the dissolution is preferably carried out under shaking conditions; the shaking speed is preferably 150-200rpm, more preferably 180rpm; the dissolution time is preferably 10-30min, more preferably 15-25min, and more preferably 20min.

[0062] Then add polysaccharide to dissolve; the polysaccharide is the same as described above and will not be repeated here; the dissolution temperature is preferably 37°C; the dissolution is preferably carried out under shaking conditions; the shaking speed is preferably 150-200rpm, more preferably 180rpm; the dissolution time is preferably 0.5-1.5h, more preferably 1h.

[0063] Add lipid nanoparticles and continue mixing; the lipid nanoparticles are preferably added in the form of an aqueous suspension; the concentration of the lipid nanoparticles in the aqueous suspension is preferably 10-500 μg / mL, more preferably 50-300 μg / mL, more preferably 50-200 μg / mL, more preferably 50-150 μg / mL, and most preferably 100 μg / mL; the mixing temperature is preferably 37° C.; the mixing is preferably carried out under shaking conditions; the shaking speed is preferably 150-200 rpm, more preferably 180 rpm; the mixing time is preferably 0.5-1.5 h, more preferably 1 h.

[0064] After mixing, the mixture is allowed to stand at low temperature and cross-linked with a calcium salt solution to obtain a hydrogel with photothermal antibacterial properties; the temperature of the low-temperature standing is preferably 0°C to 8°C, more preferably 2°C to 6°C, and more preferably 4°C; the time of the low-temperature standing is preferably 0.5 to 1.5 hours, more preferably 1 hour; the concentration of the calcium salt solution is preferably 1% to 5%, more preferably 2% to 3%; after cross-linking, ultrapure water is preferably used for washing; the number of washings is preferably three times.

[0065] The present invention also provides a cosmetic comprising the above-mentioned hydrogel with photothermal antibacterial properties.

[0066] In order to further illustrate the present invention, a hydrogel with photothermal antibacterial properties and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments.

[0067] The reagents used in the following examples are all commercially available. The experimental methods in the following examples are conventional methods unless otherwise specified. The test materials used in the following examples are purchased from conventional biochemical reagent stores unless otherwise specified. The x% in the following examples is the mass percentage unless otherwise specified. The quantitative tests in the following examples are repeated three times, and the results are averaged.

[0068] Example 1

[0069]

[0070] Anhydrous N, N-dimethylformamide (DMF, 10 mL) was added to a dry 100 mL double-necked round-bottom flask, cooled to 0 ° C and stirred, and phosphorus oxychloride (POCl3, 2 mL) was added with a syringe under argon protection. After 2 hours, dry 1,2-dichloroethane (20 mL) containing compound 1 (380 mg, 0.334 mmol) was added. Reflux overnight. After cooling to room temperature, 100 ml of water was added to quench the reaction. The mixture was extracted with dichloromethane, the organic layer was collected, washed with water, and dried over anhydrous sodium sulfate. After removing the solvent under reduced pressure, column chromatography purification (petroleum ether / dichloromethane (v / v=15 / 1)) was obtained to obtain a yellow solid compound 2 (278 mg, 70%).

[0071] Compound 2 (50 mg, 0.041 mmol) and compound 2FIC (50 mg, 0.215 mmol) were added to a double-necked flask in sequence. After pumping three times, chloroform (20 mL) was added under Ar and stirred for 5 min to completely dissolve the two compounds. Pyridine (0.5 mL) was then added and the solution slowly turned green. The mixture was refluxed at 65 ° C for 24 hours, and most of the solvent was evaporated after cooling. The crude product was then washed with methanol to remove excess compound 2FIC, and a dark blue solid compound 3 was obtained by column chromatography (petroleum ether / dichloromethane (v / v=1 / 1)) and was recorded as BTP-Th (0.309 g, yield: 90%).

[0072] The compound 3 obtained in Example 1 was analyzed by mass spectrometry to obtain its mass spectrum as shown in Figure 1 As shown, the result MS (MALDI-TOF) m / z: [M+H] + calcd.for (C 92 H 100 F4N8O2S6):1617.6308; Found:1617.6257.

[0073] Example 2

[0074] 0.3 mL of BTP-Th THF solution (1 mg / mL) was mixed with 0.1875 mL of DSPE-PEG 2000 (16 mg / mL, dissolved in THF) and mixed well. The resulting mixture was quickly added to 10 mL of deionized water, ultrasonicated in an ultrasonic bath for 2 h, and heated to remove THF and excess water to obtain lipid nanoparticles, which were recorded as BTP-Th NPs.

[0075] The lipid nanoparticles obtained in Example 2 were detected using a transmission electron microscope, and the transmission electron microscope image thereof was as follows: Figure 2 shown.

[0076] The UV-visible absorption spectrum of the BTP-Th nanoparticle (BTP-Th NPs) solution was tested using a UV-visible absorption spectrometer. The test wavelength was set to 200-1000 nm and the scanning speed was medium. The (BTP-Th NPs) solution was diluted to 10 μg / mL and placed in a quartz cuvette for testing.

[0077] Determination of BTP-Th NPs concentration and light intensity dependence: 800 mW / cm 2 The BTP-Th NPs dispersions with different concentrations (12.5, 25, 50, 100 μg / mL) were irradiated with near-infrared laser for 5 min, and the temperature change was recorded every 30 s. Under the same conditions, ultrapure water was used as the experimental control group. Different laser power densities (0.5, 0.75, 1.0, 1.5 W / cm 2 ) irradiated with ultrapure water as the control group. The trend diagram of BTP-Th NPs photothermal material changing light intensity with fixed concentration and changing concentration and temperature with fixed light intensity is obtained, as shown in the figure. Figure 3 shown.

[0078] Cyclic stability experiment of BTP-Th NPs to determine the photothermal stability: at a power density of 1 W / cm 2 100 μL BTP-Th NPs aqueous dispersion (10 μg / mL) was irradiated with 808 nm near-infrared laser for 5 min, and the temperature change was measured every 30 s. After the laser irradiation was turned off, the temperature change data was recorded again at the same time interval, with an interval of 5 min, and the on / off cycle was repeated 5 times. The photothermal stability test diagram of BTP-Th NPs photothermal material was obtained as shown in the figure below: Figure 4 shown.

[0079] The photothermal conversion efficiency of BTP-Th NPs was calculated, and the photothermal conversion diagram of BTP-Th NPs photothermal material was obtained as shown in Figure 5 shown.

[0080] η is calculated by formula (1)

[0081]

[0082] A represents the surface area of ​​the container, h represents the heat transfer coefficient. A808 is the absorbance value of the nanoparticles at 808 nm, I is the incident laser power (800 mW / cm 2 ), T Max is the maximum steady-state temperature, T Surr is the ambient temperature of the surrounding environment. S Given by the slope of the negative natural logarithm of the temperature change during cooling, τ S The value of is derived from formula (2):

[0083]

[0084] Where τ is the cooling time point after continuous irradiation, and Tt is the temperature value at the corresponding time point in the cooling process. A From formula (3), we can calculate:

[0085]

[0086] Where m D and c D Denote mass and heat capacity respectively. Dis is the heat dissipation of the solvent and the quartz sample cell, which can be calculated by formula (4):

[0087]

[0088] TMax(water) is the maximum steady-state temperature of ultrapure water.

[0089] Antibacterial experiment of BTP-Th NPs:

[0090] 1) Microbial culture

[0091] LB (Luria-Bertani) solid agar plates were used to separate Amp r A single colony of E. coli was added with 50 μg / mL ampicillin and transferred to LB (10 mL) liquid culture; cultured at 37°C for 6-12 h, centrifuged (7100 rpm, 3 min), and washed twice with phosphate buffered saline (1×PBS, pH=7.4); the resulting Amp r E. coli was resuspended in sterile 1× PBS and diluted to a suspension with an optical density of 1.0 at 600 nm (OD 600 =1.0); Similarly, MRSA and S. aureus were cultured in LB and NB (Nutrient Broth) medium, respectively, to prepare MRSA and S. aureus OD600 =1.0 of microbial suspension.

[0092] 2) Evaluation of antibacterial activity of BTP-Th NPs

[0093] 20 μL Amp r E.coli (OD 600 =1.0) and different concentrations of BTP-Th NPs (0, 5, 7.5, 10 μg / mL) were incubated at 37°C in the dark for 30 min. r The E. coli suspension was placed in the dark or irradiated with 808 nm laser at an irradiance of 550 mW / cm 2 , irradiated for 5 min; PBS solution was used to dilute 5×10 4 times; 100 μL of the dilution was spread on a solid agar plate of LB and incubated at 37°C for 16 to 18 hours to form colonies; MRSA and S. aureus and Amp r The operation of E. coli was the same, and NB was selected on the solid agar plate of S. aureus; the inhibition rate (IR) was determined as follows:

[0094] IR=(C-C0) / C0×100%

[0095] Where C is the colony forming unit (CFU) of the experimental group, and C0 is the colony forming unit number of the control group.

[0096] 3) Scanning electron microscopy (SEM) characterization

[0097] BTP-Th NPs and Amp treated in the same way as the antibacterial experiment r The E. coli mixture was centrifuged (10,000 rpm, 10 min), 100 μL 2.5% pentanediol was added to the precipitate, and fixed at 4°C overnight; the precipitate was taken out, centrifuged at 10,000 rpm for 10 min, and then resuspended in 100 μL 1× PBS, centrifuged (10,000 rpm, 10 min), and 10 μL 1× PBS was added to the precipitate and mixed; 5 μL Amp r The E. coli suspension was placed on a clean silicon wafer, washed twice with sterile water, and then 40%, 70%, 90%, and 100% ethanol were added respectively, eluted for 6 minutes, and gradient dehydration was completed. The samples were dried and then measured. The operation steps for MRSA and S. aureus were the same.

[0098] The antibacterial rate of BTP-Th NPs photothermal material against Escherichia coli and the plate graph are shown in the figure below. Figure 6 shown.

[0099] Hemolysis experiment of BTP-Th NPs:

[0100] Take 1mL of fresh rabbit blood and centrifuge at 5000rpm for 10 min to remove the supernatant and intermediate white blood cells; take 20μL of blood cell sediment and add 980μL of normal saline to prepare a 2% red blood cell solution. Add 20μL Triton X100 to the positive control group, and the negative control solvent is normal saline; add the same proportion of BTP-Th NPs dispersion solution to the experimental group, mix well and let stand for 3h; centrifuge at 10,000rpm for 2min, collect the supernatant in a 96-well plate to detect the absorbance value at 541nm. The hemolysis rate (%) is calculated as follows:

[0101]

[0102] Where I is the absorbance of the sample itself, I0 is the absorbance of the negative control, and I'' is the absorbance of the positive control.

[0103] The BTP-Th NPs photothermal material hemolysis experiment was obtained as follows Figure 7 shown.

[0104] Example 3

[0105] 0.1 g of gelatin was added to 2.5 mL of 1×PBS and dissolved in a shaker at 37°C and 180 rpm for 20 min; after dissolution, 0.05 g of sodium alginate was added and dissolved in a shaker at 37°C and 180 rpm for 1 h; 250 μL of BTP-Th NPs (100 μg / mL) obtained in Example 2 was added and dissolved in a shaker at 37°C and 180 rpm for 1 h; placed in a 24-well plate, 0.5 mL / well, refrigerated at 4°C for 1 h; soaked in 2% calcium chloride solution, washed three times with ultrapure water to obtain BTP-Th hydrogel.

[0106] Determination of the temperature-raising ability of BTP-Th hydrogel:

[0107] Using 500mW / cm 2 The BTP-Th hydrogel (BTP-Th concentration 10 μg / mL) was irradiated with a near-infrared laser of 800 mW / cm2. The temperature change data was recorded every 1 min until the temperature change region was flat. Under the same conditions, the hydrogel without BTP-Th NPs was used as the experimental control group. 2 The BTP-Th hydrogel (10 μg / mL) was irradiated with a near-infrared laser of a power density of 500 mW / cm2, and the temperature change data was recorded every 1 min until the temperature change region was flat. Under the same conditions, the hydrogel without BTP-Th NPs was used as the experimental control group. 2 and 800mW / cm 2 The light and heat change diagram under Figure 8shown.

[0108] Determination of water content of BTP-Th hydrogel:

[0109] Experimental method: The hydrogel was placed in a culture dish and two sets of parallel experiments were carried out. The culture dish weights w0=7.8323, w1=7.8684 and the hydrogel weights w2=0.4969, w3=0.4955 were weighed respectively, and then placed in a -80°C refrigerator for one night. After the hydrogel was completely frozen, it was placed in a freeze dryer for freeze drying. After freeze drying for 48 hours, the water content was calculated by weighing w4=7.8618, w5=7.8951.

[0110]

[0111] Take the average of the two moisture contents: moisture content = (moisture content 1 + moisture content 2) / 2 = (94.06% + 94.61%) / 2 = 94.34%.

[0112] Experimental results: The calculated water content of the hydrogel is 94.34%. The water content of hydrogel masks on the market is usually around 70%, which means that the water content of the hydrogel prepared by the present invention is higher than that of the masks on the market.

[0113] Determination of skin moisturizing properties of BTP-Th hydrogel:

[0114] Experimental method: Three volunteers were selected, and their forearms were washed and left to stand for 30 minutes to measure the skin moisture content. Four hydrogels were applied on the forearms of the three volunteers respectively. One hydrogel was removed every 15 minutes and the moisture content of the hydrogel-applied area was measured. After 60 minutes, the last hydrogel on the volunteer's forearm was removed and the moisture content was measured. The average value of the data of the three volunteers was taken to draw a graph.

[0115] 0min water content volunteer 1: 35.20, volunteer 2: 35.20, volunteer 3: 30.17;

[0116] 15min water content: Volunteer 1: 114.93, Volunteer 2: 103.47, Volunteer 3: 116.60;

[0117] 30min water content: volunteer 1: 115.57, volunteer 2: 105.07, volunteer 3: 118.33;

[0118] 45min water content: Volunteer 1: 118.63, Volunteer 2: 115.27, Volunteer 3: 120.00;

[0119] 60min water content: Volunteer 1: 119.80, Volunteer 2: 120.00, Volunteer 3: 120.00;

[0120] Calculate the average value of the volunteers' skin water content every 15 minutes:

[0121] 0min water content: (35.20+35.20+30.17) / 3=22.52±2.90;

[0122] 15min water content: (114.93+103.47+116.60) / 3=111.67±7.15;

[0123] 30min water content: (115.57+105.07+118.33) / 3=112.99±7.00;

[0124] 45min water content: (118.63+115.27+120.00) / 3=117.97±2.43;

[0125] Water content at 60 min: (119.80+120.00+120.00) / 3=119.93±0.12.

[0126] Experimental results: The average value of skin water content of volunteers every 15 minutes is obtained as a bar graph. Fig. 9 The experiment found that when the hydrogel was applied to the skin for 15 minutes, the water content of the skin increased significantly. As time went by, the water content of the skin continued to increase, but the increase was slow.

[0127] Water retention test of BTP-Th hydrogel:

[0128] Experimental method: After weighing three pieces of hydrogel separately, the three hydrogels were placed in a container and exposed to air at room temperature. They were weighed separately every 10 minutes. The experiment lasted for 2 hours. The water loss rate of the hydrogel was calculated as 1-z1 / z0×100%, and the average values ​​of the three groups were taken to draw the graph.

[0129] 0min glue weight: 0.5117, 0.4413, 0.4800;

[0130] 10min glue weight: 0.4458, 0.3847, 0.4372; water loss rate: 12.88%, 12.83%, 8.92%;

[0131] 20min glue weight: 0.4282, 0.3667, 0.4230; water loss rate: 16.32%, 16.90%, 11.88%;

[0132] 30min glue weight: 0.4051, 0.3432, 0.3916; water loss rate: 20.83%, 22.23%, 18.42%;

[0133] 40min glue weight: 0.3887, 0.3283, 0.3759; water loss rate: 24.04%, 25.61%, 21.69%;

[0134] 50min glue weight: 0.3761, 0.3152, 0.3607; water loss rate: 26.50%, 28.57%, 24.85%;

[0135] 60min glue weight: 0.3609, 0.2985, 0.3457; water loss rate: 29.47%, 32.36%, 27.98%;

[0136] 70min glue weight: 0.3473, 0.2854, 0.3457; water loss rate: 32.13%, 35.33%, 30.48%;

[0137] 80min glue weight: 0.3320, 0.2724, 0.3337; water loss rate: 35.12%, 38.27%, 33.13%;

[0138] 90min glue weight: 0.3226, 0.2626, 0.3061; water loss rate: 36.96%, 40.49%, 36.23%;

[0139] 100min glue weight: 0.3107, 0.2517, 0.2959; water loss rate: 39.28%, 42.96%, 38.35%;

[0140] 110min glue weight: 0.3015, 0.2442, 0.2860; water loss rate: 41.08%, 44.66%, 40.42%;

[0141] 120min glue weight: 0.2909, 0.2345, 0.2765; water loss rate: 43.15%, 46.86%, 42.40%.

[0142] The average water loss rates from 10 min to 120 min were 11.54% ± 2.272, 15.03% ± 2.750, 20.49% ± 1.929, 23.78% ± 1.972, 26.64% ± 1.864, 29.94% ± 2.227, 32.64% ± 2.465, 35.51% ± 2.596, 37.89% ± 2.282, 40.20% ± 2.438, 42.05% ± 2.285, and 44.14% ± 2.390.

[0143] Experimental results: The curve of water loss rate of hydrogel over time is as follows Fig.10 As shown. Fig.10 It can be seen that when the hydrogel is exposed to air for 2 hours at room temperature, the water loss accounts for 44.14% of the original mass, and the hydrogel still contains 50.20% of water, indicating that the hydrogel has good water retention.

[0144] Hemolytic test of BTP-Th hydrogel:

[0145] Experimental method: First, centrifuge 1mL of rabbit blood, discard the supernatant and middle layer, take 20μL of precipitate and 980μL of saline to obtain 2% red blood cell solution, 1mL of 2% red blood cell solution and 20μL of saline were mixed as negative control group, 1mL of 2% red blood cell solution and 20μL of Triton×100 were mixed as positive control group, 1g of hydrogel was prepared in a centrifuge tube, and 1.02mL of 2% red blood cells were added after gelation as experimental group. The experimental group, negative control group and positive control group were made into three groups respectively, mixed and allowed to stand for 3h, and the supernatant was taken after centrifugation to measure the absorption at 541nm. The hemolysis rate was calculated as follows:

[0146]

[0147] Where I is the absorbance of the sample itself, I0 is the absorbance of the negative control, and I'' is the absorbance of the positive control.

[0148] Experimental results: The hydrogel hemolysis rate test results are shown in the figure below: Fig.11 The hemolysis rate of the hydrogel is 0.6439%, which is much less than 5%, and has good blood compatibility.

[0149] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A hydrogel with photothermal antibacterial properties, characterized in that: It comprises a hydrogel matrix and lipid nanoparticles loaded on the hydrogel; the lipid nanoparticles contain a compound represented by formula (I); 2. The hydrogel according to claim 1, characterized in that The hydrogel matrix is ​​formed by cross-linking protein substances and polysaccharide substances; the mass ratio of the protein substances to the polysaccharide substances is 1: (0.1-1).

3. The hydrogel according to claim 2, characterized in that The protein substance is selected from gelatin and / or silk fibroin; the polysaccharide substance is selected from one or more of alginate, hyaluronic acid and chitosan.

4. The hydrogel according to claim 1, characterized in that The lipid nanoparticles include phospholipid polyethylene glycol and / or phospholipid polyethylene glycol derivatives.

5. The hydrogel according to claim 1, characterized in that The mass ratio of the hydrogel matrix to the lipid nanoparticles is 1:(0.00001-0.0005).

6. A method for preparing a hydrogel with photothermal antibacterial properties, characterized in that: The following steps are involved: The protein substance is dissolved in an aqueous solution, and then a polysaccharide substance is added and dissolved, and then lipid nanoparticles are added and mixed continuously, and the mixture is allowed to stand at low temperature, and cross-linked with a calcium salt solution to obtain a hydrogel having photothermal antibacterial properties; the lipid nanoparticles contain a compound represented by formula (I); 7. The preparation method according to claim 6, characterized in that: The compound represented by formula (I) is prepared according to the following method: S1) reacting N,N-dimethylformamide with phosphorus oxychloride at low temperature, then adding the compound represented by formula (II) for reflux reaction to obtain the compound represented by formula (III); S2) reacting the compound represented by formula (III) with the compound represented by formula (IV) in a protective atmosphere to obtain the compound represented by formula (I); 8. The preparation method according to claim 6, characterized in that: The lipid nanoparticles are prepared according to the following method: Mixing an organic solution containing a compound represented by formula (I) and an organic solution containing a phospholipid compound to obtain a mixed solution; The mixed solution was added into water and sonicated to obtain lipid nanoparticles.

9. A cosmetic, characterized in that: The invention comprises the hydrogel with photothermal antibacterial properties as claimed in any one of claims 1 to 5 or the hydrogel with photothermal antibacterial properties prepared by any one of the preparation methods of claims 6 to 8.

10. Use of the compound represented by formula (I) in preparing a hydrogel having photothermal antibacterial properties;

Citation Information

Cited By

  • Photo-thermal nanoparticle PT6 NPs and application thereof in preparation of temperature-sensitive hydrogel

    CN120714029A