Preparation method of multifunctional composite film with one-way moisture conduction and photo-thermal and drug synergistic antibacterial functions
Through electrospinning technology, a multi-layer nanofiber composite film with pore size gradient and wetting gradient is constructed. Combined with photothermal and pH-responsive controlled release drugs, the problems of existing dressings are solved, and the composite film is achieved. Antibacterial properties and one-way guide wet function avoid adhesions and provide a good healing environment.
Patent Information
- Application Number
- CN202410949059.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Existing medical dressings are difficult to effectively guide wet and antibacterial when treating wounds, and are prone to adhesions to the wounds, resulting in poor healing environment.
Through electrospinning technology, a multi-layer nanofiber composite membrane with pore size gradient and wetting gradient is constructed. Combined with photothermal effect and pH response controlled release drug function, a multi-functional composite membrane with one-way guided wet and photothermal and drug-coordinated antibacterial treatment should be formed to prevent Adhesive and achieves long-term and effective antibacterial effects.
实现了复合膜的优异抗菌性能和单向导湿功能,避免了伤口与敷料的粘连,提供了良好的愈合环境,且工艺简单、绿色安全,便于大规模生产。
Smart Images

Figure CN118903518A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a method for preparing a multifunctional composite film with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties, belonging to the technical field of special auxiliary materials or absorbent pads for surgical suture or vascular dressing. Background Art
[0002] Skin trauma is a common problem in clinical practice, among which infiltration and infection caused by wound exudate and bacterial colonization are important reasons that hinder wound healing. Although conventional medical dressings can absorb some of the exudate from wound tissue, it is inevitable that fluid will accumulate between the wound and the dressing due to material or structural reasons, repeatedly infiltrating the wound and affecting wound healing. In addition, conventional medical dressings have limited inhibitory effects on bacteria and are prone to cause adhesion between the wound and the dressing.
[0003] In the prior art, a dressing with a one-way moisture-conducting function can be constructed by designing structures and materials using a hydrophobic / hydrophilic gradient structure and a differential capillary effect. However, the research mainly focuses on the one-way moisture-conducting performance, without paying attention to the antibacterial function of the dressing. The one-way moisture-conducting dressing with antibacterial function simply loads the drug into the material and cannot effectively control the release of the drug, resulting in problems such as unstable antibacterial performance and poor durability of the dressing. At the same time, when there is a bacterial biofilm at the wound, the drug is blocked by the biofilm and is difficult to reach the wound, and the treatment effect cannot be achieved.
[0004] Therefore, in order to maintain a good healing environment for the wound, it is particularly important to develop a medical dressing that combines unidirectional moisture conduction, photothermal / drug synergistic intelligent antibacterial function, and anti-adhesion. Summary of the invention
[0005] In view of this, the present application provides a method for preparing a multifunctional composite membrane with unidirectional moisture conduction and synergistic antibacterial effects of photothermal and drugs. A multilayer nanofiber composite membrane with pore size gradient and wetting gradient is constructed by electrospinning technology. No post-treatment is required, and the process is simple and green. The hydrophilic layer of the prepared composite membrane has photothermal effect and pH-responsive controlled-release drug function. It kills bacteria by rapid temperature rise under photothermal action, and the drug controls long-term, effective and intelligent antibacterial effects. The synergistic effect of the two gives the composite membrane excellent antibacterial properties. The difference in structure and performance between the hydrophobic layer and the hydrophilic layer forms a wetting gradient effect and a differential capillary effect, giving the composite membrane excellent unidirectional moisture conduction function, and the hydrophobic layer in contact with the skin can effectively prevent the composite membrane from adhering to the wound.
[0006] Specifically, the present application is implemented through the following scheme: A method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties, comprising the following steps: Step 1: polycaprolactone, hexafluoroisopropanol solution, tannic acid, and ferric chloride hexahydrate are uniformly stirred to obtain a spinning precursor solution, and the spinning precursor solution is electrospun to obtain a hydrophilic layer nanofiber membrane, wherein the hydrophilic layer nanofiber membrane has a photothermal effect and a pH-responsive controlled-release drug function; Step 2: polycaprolactone, hexafluoroisopropanol and deionized water are mixed to obtain a polycaprolactone solution, and the polycaprolactone solution is deposited on the surface of the hydrophilic layer nanofiber membrane through electrospinning technology to form a hydrophobic layer nanofiber membrane. The hydrophilic layer nanofiber membrane and the hydrophobic layer nanofiber membrane constitute a multifunctional composite membrane with unidirectional moisture conduction and synergistic antibacterial properties of light, heat and drugs.
[0007] Further, as a preference: In step one: The molar concentration ratio of tannic acid to iron ions is 5:1-1:5, and more preferably the molar concentration ratio of tannic acid to iron ions is 3:1-1:3.
[0008] The concentration of the tannic acid solution is 1-5 wt %, more preferably, the concentration of the tannic acid solution is 1.5-3 wt %.
[0009] The hydrophilic layer nanofiber membrane has a thickness of 25-50 mm and an average pore size of 0.5-0.75 mm.
[0010] When preparing the spinning precursor solution, polycaprolactone is first dissolved in hexafluoroisopropanol solution, and then tannic acid and ferric chloride hexahydrate are added in sequence.
[0011] In step 2: The hydrophobic layer nanofiber membrane has a thickness of 2-20 mm and an average pore size of 1.5-2.5 mm.
[0012] In a polycaprolactone solution, a mixed solution of hexafluoroisopropanol and deionized water is first prepared, and then polycaprolactone is dissolved in the mixed solution to obtain a polycaprolactone solution.
[0013] The multifunctional composite film is used as a dressing for bacterially infected wounds.
[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) The hydrophilic layer and the hydrophobic layer of the multifunctional composite membrane of the present invention are both prepared by electrospinning process, which has simple steps and is easy to operate; (2) The present invention can effectively control the hydrophilicity and hydrophobicity and pore size of the hydrophilic layer and hydrophobic layer of the multifunctional composite membrane by changing the material composition, ratio and electrospinning time, thereby obtaining an excellent differential capillary effect and wettability gradient effect, and realizing a unidirectional moisture conduction function; (3) The multifunctional composite membrane of the present invention has tannic acid loaded on the hydrophilic layer and iron ions self-assembled to form a complex, which gives the hydrophilic layer a photothermal effect and a pH-responsive controlled-release drug function. It can be quickly sterilized by heating under the photothermal effect, and the pH responsiveness can control the release of the antibacterial agent tannic acid based on the wound microenvironment; the hydrophobic layer nanofiber membrane can effectively prevent the wound from adhering to the dressing; The multifunctional composite membrane prepared by the above scheme integrates photothermal and drug antibacterial functions and unidirectional moisture conduction functions. The preparation method is simple, green and safe, can be convenient for large-scale production, and can be widely used in wounds infected with bacteria and bacterial biofilms. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is an electron microscope image of the multifunctional composite membrane prepared in Example 1 of the present application; Figure 2 The pore size distribution of each layer of fiber membrane in the multifunctional composite membrane prepared in Example 1 of the present application; Figure 3 The photothermal effect of each layer of fiber membrane in the multifunctional composite membrane prepared in Example 1 of the present application; Figure 4 The drug release behavior under pH response of the multifunctional composite membrane prepared in Example 1 of the present application; Figure 5 The antibacterial properties of the multifunctional composite membrane prepared in Example 1 of the present application; Figure 6 The unidirectional moisture conduction performance of the multifunctional composite membrane prepared in Example 1 of the present application; Figure 7 The water contact angle of the multifunctional composite membrane prepared in Example 1 of the present application; Figure 8 The water contact angle changes of the multifunctional composite membranes prepared in Examples 1, 2, and 3 of the present application. Specific implementation methods
[0016] Example 1
[0017] (1) Polycaprolactone was dissolved in hexafluoroisopropanol to prepare a 10 wt% polymer solution, and tannic acid and ferric chloride hexahydrate were added thereto in sequence, wherein the mass fraction of tannic acid was 2 wt% and the molar ratio of tannic acid to ferric chloride hexahydrate was 1:1. A magnetic stirrer was used to stir at 25 °C for 24 hours to form a uniform spinning solution. A hydrophilic nanofiber membrane with photothermal effect and pH response was prepared by electrospinning technology. The electrospinning parameters were as follows: spinning voltage 13 kV, needle model 18 G, spinning solution flow rate 0.5 mL h -1 , the receiving distance is 15 cm, the average fiber diameter is 280 nm, the average pore size is 0.6 mm, and the membrane thickness is 35 mm; (2) According to the concentration ratio of 10 wt%, polycaprolactone was dissolved in a mixed solution of hexafluoroisopropanol and deionized water (hexafluoroisopropanol: deionized water = 75:25), and stirred with a magnetic stirrer at 25 °C for 24 hours to form a uniform spinning solution. The spinning solution was deposited on the surface of the hydrophilic layer obtained in the above step (1) by electrospinning technology to obtain a hydrophobic nanofiber membrane. The electrospinning parameters were: spinning voltage 15 kV, needle model 18G, spinning solution flow rate 0.5 mL h -1 , the receiving distance is 15 cm, the average fiber diameter is 930 nm, the average pore size is 2.0 mm, and the membrane thickness is 10 mm.
[0018] Example 2
[0019] (1) Polycaprolactone was dissolved in hexafluoroisopropanol to prepare a 10 wt% polymer solution, and tannic acid and ferric chloride hexahydrate were added thereto in sequence, wherein the mass fraction of tannic acid was 2 wt% and the molar ratio of tannic acid to ferric chloride hexahydrate was 1:1. A magnetic stirrer was used to stir at 25 °C for 24 hours to form a uniform spinning solution. A hydrophilic nanofiber membrane with photothermal effect and pH response was prepared by electrospinning technology. The electrospinning parameters were as follows: spinning voltage 13 kV, needle model 18 G, spinning solution flow rate 0.5 mL h -1 , the receiving distance is 15 cm, the average fiber diameter is 280 nm, the average pore size is 0.6 mm, and the membrane thickness is 35 mm; (2) Polycaprolactone was dissolved in hexafluoroisopropanol and deionized water (hexafluoroisopropanol: deionized water = 75:25) at a concentration ratio of 10 wt%, and stirred with a magnetic stirrer at 25 °C for 24 hours to form a uniform spinning solution. A hydrophobic nanofiber membrane was deposited on the surface of the hydrophilic layer obtained in the above step (1) by electrospinning technology. The electrospinning parameters were as follows: spinning voltage 15 kV, needle model 18 G, spinning solution flow rate 0.5 mL h -1 , the receiving distance is 15 cm, the average diameter of the obtained fiber is 930 nm, the average pore size is 2.0 mm, and the membrane thickness is 15 mm.
[0020] Example 3
[0021] (1) Polycaprolactone was dissolved in hexafluoroisopropanol to prepare a 10 wt% polymer solution, and tannic acid and ferric chloride hexahydrate were added thereto in sequence, wherein the mass fraction of tannic acid was 2 wt% and the molar ratio of tannic acid to ferric chloride hexahydrate was 1:1. A magnetic stirrer was used to stir at 25 °C for 24 hours to form a uniform spinning solution. A hydrophilic nanofiber membrane with photothermal effect and pH response was prepared by electrospinning technology. The electrospinning parameters were as follows: spinning voltage 13 kV, needle model 18 G, spinning solution flow rate 0.5 mL h -1, the receiving distance is 15 cm, the average fiber diameter is 280 nm, the average pore size is 0.6 mm, and the membrane thickness is 35 mm; (2) 10 wt% polycaprolactone was dissolved in hexafluoroisopropanol and stirred with a magnetic stirrer at 25 °C for 24 h to form a uniform spinning solution. The solution was deposited on the surface of the hydrophilic layer obtained in the above step (2) by electrospinning technology to prepare a bottom hydrophobic nanofiber membrane. The electrospinning parameters were as follows: spinning voltage 15 kV, needle type 18G, spinning solution flow rate 0.5 mL h -1 , the receiving distance is 15 cm, the average fiber diameter is 930 nm, the average pore size is 2.0 mm, and the membrane thickness is 20 mm.
[0022] The performance test was carried out using the multifunctional composite membrane obtained in Example 1 as a representative, and the results are as follows: Combination Figure 1 It can be seen from the electron microscope image that the obtained multifunctional composite membrane is composed of fibers with different diameters, and the material exhibits a multi-pore size effect.
[0023] Pore size distribution Figure 2 As shown: the pore size of the hydrophilic layer nanofiber membrane is concentrated around 0.6 mm, while the pore size of the hydrophobic layer nanofiber membrane is distributed around 2.0 mm.
[0024] The photothermal effect test results are as follows Figure 3 As shown: the temperature rises rapidly within 5 minutes, and basically stabilizes at around 47°C after 6 minutes. Sterilization is achieved by rapid temperature rise under the photothermal effect.
[0025] Drug release behavior under pH response Figure 4 As shown: at pH 5.5, the cumulative drug release quickly reaches about 65% at 7.5h, and the cumulative drug release quickly reaches about 68% at 15h; at pH 6.8, the cumulative drug release quickly reaches about 53% at 7.5h, and the cumulative drug release quickly reaches about 58% at 15h; at pH 8.5, the cumulative drug release quickly reaches about 52% at 7.5h, and the cumulative drug release increases insignificantly if the time is extended. This shows that the multifunctional composite film obtained in this case can realize drug control to achieve long-term and effective intelligent antibacterial, and synergize with the photothermal effect to give the composite film excellent antibacterial properties.
[0026] Antibacterial properties such as Figure 5 As shown: Under non-light conditions, the multifunctional composite membrane has obvious antibacterial activity against Escherichia coli and Staphylococcus aureus, and the antibacterial rate against both bacteria reaches 90%; under light conditions, the antibacterial rate of the multifunctional composite membrane is further increased to nearly 100%, which fully demonstrates that under the synergistic effect of light, heat and drugs, the multifunctional composite membrane has excellent antibacterial properties.
[0027] Combined with unidirectional moisture conduction properties such as Figure 6 As shown: when fluorescent water droplets are dropped from one side of the bottom hydrophobic layer nanofiber membrane, they can be quickly absorbed to the top layer within 20 s, while when they are dropped from one side of the top hydrophilic layer nanofiber membrane, they will not be transmitted to the other side. The differences in structure and performance between the hydrophobic layer nanofiber membrane and the hydrophilic layer nanofiber membrane form a wetting gradient effect and a differential capillary effect, which endows the multifunctional composite membrane with good unidirectional moisture conduction function.
[0028] The hydrophilic layer nanofiber membrane and the hydrophobic layer nanofiber membrane were tested separately, and the results are as follows Figure 7 As shown: the water droplet is completely immersed in the hydrophilic layer nanofiber membrane within 6 seconds, while the water droplet on the hydrophobic layer nanofiber membrane remains on the surface of the material for more than 60 seconds.
[0029] The different conditions of the above three embodiments can obtain a multilayer nanofiber composite membrane with a pore size gradient and a wettability gradient. The water contact angle changes of the multifunctional composite membranes prepared in the above three embodiments are statistically analyzed. Figure 8 As shown: after 5 mL of water droplets were dropped from one side of the hydrophobic layer nanofiber membrane, the multifunctional composite membrane obtained in Example 1 could be quickly absorbed into the top hydrophilic layer nanofiber membrane within 10 s, the multifunctional composite membrane obtained in Example 2 could be quickly absorbed into the top hydrophilic layer nanofiber membrane within 24 s, and the multifunctional composite membrane obtained in Example 3 could be quickly absorbed into the top hydrophilic layer nanofiber membrane within 30 s.
Claims
1. A method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties, characterized in that: The following steps are involved: Step 1: polycaprolactone, hexafluoroisopropanol solution, tannic acid, and ferric chloride hexahydrate are uniformly stirred to obtain a spinning precursor solution, and the spinning precursor solution is electrospun to obtain a hydrophilic layer nanofiber membrane, wherein the hydrophilic layer nanofiber membrane has a photothermal effect and a pH-responsive controlled-release drug function; Step 2: polycaprolactone, hexafluoroisopropanol and deionized water are mixed to obtain a polycaprolactone solution, and the polycaprolactone solution is deposited on the surface of the hydrophilic layer nanofiber membrane through electrospinning technology to form a hydrophobic layer nanofiber membrane. The hydrophilic layer nanofiber membrane and the hydrophobic layer nanofiber membrane constitute a multifunctional composite membrane with unidirectional moisture conduction and synergistic antibacterial properties of light, heat and drugs.
2. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: In step 1, the molar concentration ratio of tannic acid to iron ions is 5:1 to 1:
5.
3. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 2, characterized in that: The molar concentration ratio of tannic acid to iron ions is 3:1~1:
3.
4. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: In step 1, the concentration of the tannic acid solution is 1-5 wt%.
5. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 4, characterized in that: The concentration of the tannic acid solution is 1.5-3 wt %.
6. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: In step 1, the hydrophilic layer nanofiber membrane has a thickness of 25-50 mm and an average pore size of 0.5-0.75 mm.
7. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: In step 1, polycaprolactone is first dissolved in a hexafluoroisopropanol solution, and then tannic acid and ferric chloride hexahydrate are added in sequence.
8. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: In step 2, the hydrophobic layer nanofiber membrane has a thickness of 2-20 mm and an average pore size of 1.5-2.5 mm.
9. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: In step 2, a mixed solution of hexafluoroisopropanol and deionized water is first prepared, and then polycaprolactone is dissolved in the mixed solution to obtain a polycaprolactone solution.
10. The method for preparing a multifunctional composite membrane with unidirectional moisture conduction and photothermal and drug synergistic antibacterial properties according to claim 1, characterized in that: The multifunctional composite film is used as a dressing for bacterial-infected wounds.
Citation Information
Cited By
Preparation method of hydrophilic / hydrophobic double-layer nanofiber membrane with full-degradable characteristic
CN119711050A
Preparation method of hydrophilic / hydrophobic double-layer nanofiber membrane with full degradability
CN119711050B
Near-infrared-triggered phase-change controlled-release low-temperature photo-thermal synergistic nano-particles as well as preparation and application thereof
CN122163797A