Hydrogel material for preparing traumatic wound sealant as well as preparation method and application of hydrogel material

By using the esterification reaction of components such as gelatin, methacrylic anhydride and the addition of nanosilver in traumatic wound sealing agents, a hydrogel material with high adhesion strength and rapid curing was prepared, and the traumaticity in the prior art was solved. The problem of insufficient hemostasis performance of wound sealing agents has achieved rapid sealing and antibacterial effects on traumatic wounds.

CN118903524APending Publication Date: 2024-11-08GENERAL HOSPITAL OF THE NORTHERN WAR ZONE OF THE CHINESE PEOPLES LIBERATION ARMY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966161.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing traumatic wound sealing agents cannot adhere and seal quickly with continuous blood flow, especially in the aortic and cardiac trauma, which exhibit insufficient hemostasis, adhesion and mechanical strength.

Method used

Hydrogels with high adhesion strength and fast curing were prepared by esterification reactions of components such as gelatin, methacrylic anhydride, soluble starch, silver nitrate, β-D glucose and silanized hyaluronic acid under ultraviolet light. The material, combined with the antibacterial effect of nanosilver, improves the biocompatibility and mechanical properties of the material.

Benefits of technology

It achieves rapid adhesion and sealing of traumatic wounds under continuous flow, with high burst pressure, good peeling adhesion and antibacterial properties, and is suitable for hemostasis of trauma such as aorta and heart.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogel, in particular to a hydrogel material for preparing a traumatic wound sealant as well as a preparation method and application of the hydrogel material. According to the preparation method, methylacryloyl gelatin is prepared from gelatin, a first buffer solution and methacrylic anhydride, a nano-silver solution is obtained from a soluble starch aqueous solution, a silver nitrate aqueous solution and a beta-D glucose aqueous solution, the methylacryloyl gelatin and nano-silver are mixed, and methylacryloyl gelatin-nano-silver is obtained; and compounding and cross-linking with silanized hyaluronic acid and an LAP photoinitiator under ultraviolet light to form the hydrogel material. The material has good biocompatibility, mechanical strength and antibacterial property, is high in curing speed under ultraviolet light, and can achieve rapid adhesion and sealing on traumatic wounds under the condition of continuous flowing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogels, and in particular to a hydrogel material for preparing a traumatic wound sealant, and a preparation method and application thereof. Background Art

[0002] In the event of emergency trauma or surgical operation, traumatic wound sealants are often needed to stop bleeding. Currently, fibrin glue, gelatin, collagen and oxidized fibers are used for rapid wound closure. However, due to slow hemostatic performance, poor surface adhesion, insufficient mechanical strength and other reasons, the existing sealing materials are insufficient in rapid adhesion and wound sealing when blood continues to flow, making them unsuitable for hemostasis of aortic and cardiac trauma. Summary of the invention

[0003] The purpose of the present invention is to provide a hydrogel material for preparing a traumatic wound sealant, a preparation method and application thereof, which has high adhesion strength and good sealing effect.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] A method for preparing a hydrogel material for preparing a traumatic wound sealant comprises the following steps:

[0006] 1) mixing gelatin, a first buffer solution and methacrylic anhydride, and performing an esterification reaction to obtain methacrylated gelatin;

[0007] 2) mixing a soluble starch aqueous solution, a silver nitrate aqueous solution, a β-D glucose aqueous solution and the methacrylylated gelatin to obtain methacrylylated gelatin-nanosilver;

[0008] 3) mixing the methacrylylated gelatin-nanosilver, silanized hyaluronic acid, LAP photoinitiator and a second buffer solution to obtain a hydrogel precursor solution; photocuring the hydrogel precursor solution under ultraviolet light irradiation to obtain a hydrogel material for preparing a traumatic wound sealant.

[0009] Optionally, in step 1), the first buffer solution is a PBS solution; the usage ratio of gelatin to the first buffer solution is 1 g: 5-12 mL; and the usage ratio of gelatin to methacrylic anhydride is 1 g: 0.1-0.3 mL.

[0010] Optionally, the temperature of the esterification reaction in step 1) is 40-60° C. and the time is 2-5 hours.

[0011] Optionally, in step 2), the concentration of the soluble starch is 5-9 g / L; the volume ratio of the soluble starch aqueous solution to the silver nitrate aqueous solution is 50-300:0.05-0.5.

[0012] Optionally, in step 2), the concentration of the silver nitrate aqueous solution is 0.09-0.12 mol / L; the concentration of the β-D glucose aqueous solution is 0.09-0.12 mol / L; the volume ratio of the silver nitrate aqueous solution to the β-D glucose aqueous solution is 0.8-1.2:1; and the mass ratio of the soluble starch aqueous solution to the methacryloyl gelatin is 0.5-3:1-4.

[0013] Optionally, in step 3), the concentration of methacrylated gelatin-silver nanoparticles in the hydrogel precursor solution is 5 to 10 wt%, the concentration of silanized hyaluronic acid is 1 to 2.5 wt%, and the concentration of the LAP photoinitiator is 0.1 to 0.5 wt%.

[0014] Optionally, in step 3), the second buffer solution is a PBS solution; the wavelength of the ultraviolet light is 300-405 nm, and the power is 25-40 mW / cm 2 , the light curing time is 5 to 15 seconds.

[0015] The invention provides a hydrogel material prepared by the preparation method and used for preparing a traumatic wound sealant.

[0016] The present invention also provides application of the hydrogel material for preparing a traumatic wound sealant in preparing a traumatic wound sealant.

[0017] In the process of preparing the hydrogel material for preparing a traumatic wound sealant of the present invention, methacrylated gelatin combines the biocompatibility of gelatin and the photopolymerization characteristics of methacrylate, so that the hydrogel material has excellent biodegradability, biocompatibility, photopolymerization characteristics and water solubility; and methacrylated gelatin helps cells to adhere to and proliferate on its surface; and nanosilver has a spectral antibacterial effect and high antibacterial activity, and can promote wound healing and tissue repair. The addition of nanosilver improves the mechanical properties of methacrylated gelatin and promotes wound healing.

[0018] In the process of preparing the hydrogel material for preparing the traumatic wound sealant of the present invention, silanized hyaluronic acid is used. Hyaluronan has extremely high biocompatibility, can be degraded in the body, can promote cell adhesion and migration and is non-toxic; hyaluronic acid is also a natural component of the extracellular matrix, which helps to maintain the structure and function of the tissue; and silicon also exists in the extracellular matrix. The mechanical strength of the material can be improved by combining silanized hyaluronic acid with methacryloyl gelatin. In addition, silanol in silanized hyaluronic acid can simulate the morphology of natural silicon in the body, help rebuild tissues and promote cell proliferation.

[0019] The hydrogel material for preparing a traumatic wound sealant prepared by the present invention has good biocompatibility, mechanical strength and antibacterial properties and a fast curing speed under ultraviolet light, and can achieve rapid adhesion and sealing to a traumatic wound under continuous flow. DETAILED DESCRIPTION

[0020] The present invention provides a method for preparing a hydrogel material for preparing a traumatic wound sealant, comprising the following steps:

[0021] 1) mixing gelatin, a first buffer solution and methacrylic anhydride, and performing an esterification reaction to obtain methacrylated gelatin;

[0022] 2) mixing a soluble starch aqueous solution, a silver nitrate aqueous solution, a β-D glucose aqueous solution and the methacrylylated gelatin to obtain methacrylylated gelatin-nanosilver;

[0023] 3) mixing the methacrylylated gelatin-nanosilver, silanized hyaluronic acid, LAP photoinitiator and a second buffer solution to obtain a hydrogel precursor solution; photocuring the hydrogel precursor solution under ultraviolet light irradiation to obtain a hydrogel material for preparing a traumatic wound sealant.

[0024] In the present invention, in step 1), the first buffer solution is preferably a PBS solution; the usage ratio of gelatin to the first buffer solution is preferably 1 g: 5-12 mL, and more preferably 1 g: 8-10 mL; the usage ratio of gelatin to methacrylic anhydride is preferably 1 g: 0.1-0.3 mL, and more preferably 1 g: 0.125-0.2 mL, and even more preferably 0.15-0.175 mL.

[0025] In the present invention, the mixing in step 1) is preferably performed by dissolving gelatin in a first buffer solution to prepare a gelatin solution, and then adding methacrylic anhydride.

[0026] In the present invention, the temperature of the esterification reaction in step 1) is preferably 40 to 60° C., more preferably 45 to 50° C.; the time is preferably 2 to 5 hours, more preferably 3 to 4 hours.

[0027] In the present invention, after the esterification reaction is completed, a first buffer solution preheated to the reaction temperature is preferably added to stop the reaction, followed by dialysis for 7 days and drying to obtain the methacrylic anhydride powder; the drying conditions are not particularly limited, and any conditions that can achieve drying are preferred, and lyophilization at -80°C is preferred.

[0028] In the present invention, the concentration of the soluble starch in step 2) is preferably 5-9 g / L, more preferably 6-8 g / L; the volume ratio of the soluble starch aqueous solution to the silver nitrate aqueous solution is preferably 50-300:0.05-0.5, more preferably 80-200:0.1-0.4, and even more preferably 100-150:0.2-0.25.

[0029] In the present invention, the concentration of the silver nitrate aqueous solution in step 2) is preferably 0.09-0.12 mol / L, more preferably 0.1-0.11 mol / L; the concentration of the β-D glucose aqueous solution is preferably 0.09-0.12 mol / L, more preferably 0.1-0.11 mol / L; the volume ratio of the silver nitrate aqueous solution to the β-D glucose aqueous solution is preferably 0.8-1.2:1, more preferably 1-1.1:1; the mass ratio of the soluble starch aqueous solution to the methacryloyl gelatin is preferably 0.5-3:1-4, more preferably 1-2:1.5-3, and even more preferably 1.2-1.5:2-2.5.

[0030] In the present invention, the mixing in step 2) is preferably performed by first mixing the soluble starch aqueous solution, the silver nitrate aqueous solution and the β-D glucose solution; reacting at 80° C. for 30 minutes to obtain the nanosilver solution;

[0031] The nanosilver solution is cooled to 50° C., and methacrylated gelatin is added, mixed thoroughly, and dried to obtain methacrylated gelatin-nanosilver powder; the drying conditions are not particularly limited, and any conditions that can achieve drying are acceptable.

[0032] In the present invention, the method for preparing the silanized hyaluronic acid in step 3) is preferably to dissolve the hyaluronic acid solution in dimethyl sulfoxide, then add 1,1-dimethylol-silane-1-acetate and HCl with a mass concentration of 37%, react at room temperature for 24 hours, then pour the reaction solution into anhydrous ethanol, filter, wash and dry in sequence to obtain the silanized hyaluronic acid powder;

[0033] The dosage ratio of hyaluronic acid to dimethyl sulfoxide is preferably 1 g: 10 to 18 mL, and more preferably 1 g: 12 to 16 mL;

[0034] The mass ratio of hyaluronic acid to 1,1-dimethylol-silane-1-acetate is preferably 3.5 to 8:1, more preferably 4 to 7:1, and even more preferably 5 to 6:1;

[0035] The mass ratio of the hyaluronic acid to 37% HCl is preferably 50:0.5-2, more preferably 50:1-1.5;

[0036] The volume ratio of dimethyl sulfoxide to anhydrous ethanol is preferably 1:9-14, and more preferably 1:10-12; the washing solution is preferably water, and the drying conditions are not particularly limited, and any conditions that can achieve drying are acceptable.

[0037] In the present invention, the mixing temperature in step 3) is preferably 40-60°C, and more preferably 45-50°C; the mixing is preferably performed by dissolving methacrylated gelatin-nanosilver, silanized hyaluronic acid, and LAP photoinitiator in a second buffer solution respectively and then mixing them. The amounts of the second buffer solution and methacrylated gelatin-nanosilver, silanized hyaluronic acid, and LAP photoinitiator used in the dissolution process are not particularly limited, and the resulting hydrogel precursor solution can satisfy the concentration of each component.

[0038] In the present invention, the concentration of methacrylated gelatin-nanosilver in the hydrogel precursor solution in step 3) is preferably 5-10wt%, more preferably 6-9wt%, and more preferably 7-8wt%; the concentration of silanized hyaluronic acid is preferably 1-2.5wt%, more preferably 1.5-2.25wt%, and more preferably 1.75-2wt%; the concentration of LAP photoinitiator is preferably 0.1-0.5wt%, more preferably 0.2-0.4wt%, and more preferably 0.25-0.3wt%.

[0039] In the present invention, the second buffer solution in step 3) is preferably a PBS solution; the wavelength of the ultraviolet light is preferably 300 to 405 nm, more preferably 365 to 395 nm; the power is preferably 25 to 40 mW / cm 2 , more preferably 30 to 35 mW / cm 2 ; The photocuring time is preferably 5 to 15 s, more preferably 6 to 12 s, and even more preferably 8 to 10 s.

[0040] The invention provides a hydrogel material prepared by the preparation method and used for preparing a traumatic wound sealant.

[0041] The present invention also provides application of the hydrogel material for preparing a traumatic wound sealant in preparing a traumatic wound sealant.

[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0043] Example 1

[0044] Deionized water was used to prepare 0.1 mol / L silver nitrate solution; 0.1 mol / L β-D glucose solution; 8 g / L soluble starch aqueous solution; and LAP photoinitiator was purchased.

[0045] 10 g of gelatin was dissolved in 100 mL of PBS solution (purchased from Biyuntian Biotechnology Co., Ltd.) to prepare a gelatin solution, and then 1.25 mL of methacrylic anhydride was added, reacted at 50°C for 3 h, and then 50 mL of PBS solution preheated to 50°C was added. After dialysis for 7 days, the solution was freeze-dried at -80°C to obtain methacrylylated gelatin (GelMA) powder;

[0046] Mix 150 mL of 8 g / L soluble starch aqueous solution, 0.2 mL of 0.1 mol / L silver nitrate solution, and 0.2 mL of 0.1 mol / L β-D glucose solution; react at 80° C. for 30 min to obtain a nanosilver solution;

[0047] The nanosilver solution was cooled to 50° C., 2.5 g of methacryloyl gelatin (GelMA) powder was added, and the mixture was fully mixed and freeze-dried at -80° C. to obtain methacryloyl gelatin-nanosilver powder;

[0048] 5 g of hyaluronic acid solution was dissolved in 80 mL of dimethyl sulfoxide, followed by the addition of 1 g of 1,1-dimethylol-silane-1-acetate and 0.05 g of HCl with a mass concentration of 37%, and the reaction was carried out at room temperature for 24 h. The reaction solution was then poured into 800 mL of anhydrous ethanol, and then filtered, washed with deionized water, and freeze-dried at -80°C to obtain silanized hyaluronic acid powder;

[0049] At 45° C., dissolving methacrylated gelatin-nanosilver powder, silanized hyaluronic acid powder and LAP photoinitiator in PBS solution respectively and then mixing to obtain a hydrogel precursor solution; the concentration of methacrylated gelatin-nanosilver in the hydrogel precursor solution is 8wt%, the concentration of silanized hyaluronic acid is 1.5wt%, and the concentration of LAP photoinitiator is 0.25wt%;

[0050] The hydrogel precursor solution was treated with an ultraviolet light source with a wavelength of 365 nm and a power of 30 mW / cm 2 , the curing time is 10 s, and the hydrogel for preparing a traumatic wound sealant is obtained.

[0051] Example 2

[0052] Deionized water was used to prepare 0.1 mol / L silver nitrate solution; 0.1 mol / L β-D glucose solution; 8 g / L soluble starch aqueous solution; and LAP photoinitiator was purchased.

[0053] 10 g of gelatin was dissolved in 100 mL of PBS solution (purchased from Biyuntian Biotechnology Co., Ltd.) to prepare a gelatin solution, and then 1.25 mL of methacrylic anhydride was added, reacted at 50°C for 3 h, and then 50 mL of PBS solution preheated to 50°C was added. After dialysis for 7 days, the solution was freeze-dried at -80°C to obtain methacrylylated gelatin (GelMA) powder;

[0054] Mix 150 mL of 8 g / L soluble starch aqueous solution, 0.25 mL of 0.1 mol / L silver nitrate solution, and 0.25 mL of 0.1 mol / L β-D glucose solution; react at 80° C. for 30 min to obtain a nanosilver solution;

[0055] The nanosilver solution was cooled to 50° C., 4 g of methacryloyl gelatin (GelMA) powder was added, and the mixture was fully mixed and freeze-dried at -80° C. to obtain methacryloyl gelatin-nanosilver powder;

[0056] 10 g of hyaluronic acid solution was dissolved in 100 mL of dimethyl sulfoxide, followed by the addition of 2.5 g of 1,1-dimethylol-silane-1-acetate and 0.2 g of HCl with a mass concentration of 37%, and the reaction was carried out at room temperature for 24 h. The reaction solution was then poured into 900 mL of anhydrous ethanol, and then filtered, washed with deionized water, and freeze-dried at -80°C to obtain silanized hyaluronic acid powder;

[0057] At 45° C., dissolving methacrylated gelatin-nanosilver powder, silanized hyaluronic acid powder and LAP photoinitiator in PBS solution respectively and then mixing to obtain a hydrogel precursor solution; the concentration of methacrylated gelatin-nanosilver in the hydrogel precursor solution is 8wt%, the concentration of silanized hyaluronic acid is 1.5wt%, and the concentration of LAP photoinitiator is 0.25wt%;

[0058] The hydrogel precursor solution was treated with an ultraviolet light source with a wavelength of 365 nm and a power of 30 mW / cm 2 , the curing time is 6 s, and the hydrogel for preparing a traumatic wound sealant is obtained.

[0059] Example 3

[0060] Deionized water was used to prepare 0.1 mol / L silver nitrate solution; 0.1 mol / L β-D glucose solution; 8 g / L soluble starch aqueous solution; and LAP photoinitiator was purchased.

[0061] 10 g of gelatin was dissolved in 100 mL of PBS solution (purchased from Biyuntian Biotechnology Co., Ltd.) to prepare a gelatin solution, followed by adding 2 mL of methacrylic anhydride and reacting at 50 °C for 3 h, followed by adding 50 mL of PBS solution preheated to 50 °C, dialyzing for 7 days and then freeze-drying at -80 °C to obtain methacrylylated gelatin (GelMA) powder;

[0062] 150 mL of 8 g / L soluble starch aqueous solution, 0.2 mL of 0.1 mol / L silver nitrate solution and 0.2 mL of 0.1 mol / L β-D glucose solution were reacted at 80° C. for 30 min to obtain a nanosilver solution;

[0063] The nanosilver solution was cooled to 50° C., 2.5 g of methacryloyl gelatin (GelMA) powder was added, and the mixture was fully mixed and freeze-dried at -80° C. to obtain methacryloyl gelatin-nanosilver powder;

[0064] 12 g of hyaluronic acid solution was dissolved in 165 mL of dimethyl sulfoxide, followed by the addition of 2 g of 1,1-dimethylol-silane-1-acetate and 0.36 g of HCl with a mass concentration of 37%, and the reaction was carried out at room temperature for 24 h. The reaction solution was then poured into 2000 mL of anhydrous ethanol, and then filtered, washed with deionized water, and freeze-dried at -80°C to obtain silanized hyaluronic acid powder;

[0065] At 45° C., dissolving methacrylated gelatin-nanosilver powder, silanized hyaluronic acid powder and LAP photoinitiator in PBS solution respectively and then mixing to obtain a hydrogel precursor solution; the concentration of methacrylated gelatin-nanosilver in the hydrogel precursor solution is 9wt%, the concentration of silanized hyaluronic acid is 2wt%, and the concentration of LAP photoinitiator is 0.2wt%;

[0066] The hydrogel precursor solution was treated with an ultraviolet light source with a wavelength of 365 nm and a power of 30 mW / cm 2 , the curing time is 8 s, and the hydrogel for preparing a traumatic wound sealant is obtained.

[0067] Comparative Example 1

[0068] LAP photoinitiator was purchased.

[0069] 10 g of gelatin was dissolved in 100 mL of PBS solution (purchased from Biyuntian Biotechnology Co., Ltd.) to prepare a gelatin solution, and then 1.25 mL of methacrylic anhydride was added, reacted at 50°C for 3 h, and then 50 mL of PBS solution preheated to 50°C was added. After dialysis for 7 days, the solution was freeze-dried at -80°C to obtain methacrylylated gelatin (GelMA) powder;

[0070] 5 g of hyaluronic acid solution was dissolved in 80 mL of dimethyl sulfoxide, followed by the addition of 1 g of 1,1-dimethylol-silane-1-acetate and 0.05 g of HCl with a mass concentration of 37%, and the reaction was carried out at room temperature for 24 h. The reaction solution was then poured into 800 mL of anhydrous ethanol, and then filtered, washed with deionized water, and freeze-dried at -80°C to obtain silanized hyaluronic acid powder;

[0071] At 45° C., dissolving methacrylated gelatin powder, silanized hyaluronic acid powder and LAP photoinitiator in PBS solution respectively and then mixing to obtain a hydrogel precursor solution; the concentration of methacrylated gelatin in the hydrogel precursor solution is 8wt%, the concentration of silanized hyaluronic acid is 1.5wt%, and the concentration of LAP photoinitiator is 0.25wt%;

[0072] The hydrogel precursor solution was treated with an ultraviolet light source with a wavelength of 365 nm and a power of 30 mW / cm 2 , the curing time is 10 s, and the hydrogel for preparing a traumatic wound sealant is obtained.

[0073] Comparative Example 2

[0074] Deionized water was used to prepare a 0.1 mol / L silver nitrate solution; 0.1 mol / L β-D glucose solution LAP photoinitiator was purchased.

[0075] 10 g of gelatin was dissolved in 100 mL of PBS solution (purchased from Biyuntian Biotechnology Co., Ltd.) to prepare a gelatin solution, and then 1.25 mL of methacrylic anhydride was added, reacted at 50°C for 3 h, and then 50 mL of PBS solution preheated to 50°C was added. After dialysis for 7 days, the solution was freeze-dried at -80°C to obtain methacrylylated gelatin (GelMA) powder;

[0076] 1.2 g of soluble starch was added to 150 mL of deionized water, followed by 0.2 mL of 0.1 mol / L silver nitrate solution and 0.2 mL of 0.1 mol / L β-D glucose solution; the reaction was carried out at 80° C. for 30 min to obtain a nanosilver solution;

[0077] The nanosilver solution was cooled to 50° C., 2.5 g of methacryloyl gelatin (GelMA) powder was added, and the mixture was fully mixed and freeze-dried at -80° C. to obtain methacryloyl gelatin-nanosilver powder;

[0078] At 45° C., dissolving methacrylated gelatin-nanosilver powder, hyaluronic acid powder and LAP photoinitiator in PBS solution respectively and then mixing to obtain a hydrogel precursor solution; the concentration of methacrylated gelatin-nanosilver in the hydrogel precursor solution is 8wt%, the concentration of hyaluronic acid is 1.5wt%, and the concentration of LAP photoinitiator is 0.25wt%;

[0079] The hydrogel precursor solution was treated with an ultraviolet light source with a wavelength of 365 nm and a power of 30 mW / cm 2 , the curing time is 10 s, and the hydrogel for preparing a traumatic wound sealant is obtained.

[0080] Test Case

[0081] The bursting pressure, peeling adhesion and antibacterial property of the hydrogels for preparing traumatic wound sealants prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested respectively:

[0082] 1. Burst pressure test

[0083] Fresh intestinal membrane tissue was fixed to a syringe pump (containing PBS solution), and after incision was made on the surface of the intestinal membrane tissue, 500 μl of the hydrogel precursor solution prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were injected into the incision, and then irradiated with ultraviolet light (ultraviolet light source with a wavelength of 365 nm and a power of 30 mW / cm 2 ) After 20 s, the injection pump was pressurized to perform a burst pressure test, and the highest pressure reached by the injection pump before the hydrogel ruptured was taken as the burst pressure. The results are shown in Table 1;

[0084] 2. Peel Adhesion Test

[0085] Use porcine small intestine membrane, bond it to a piece of PET film with CA adhesive and leave one end of the PET film unbonded to limit the deformation of the crack tip;

[0086] The hydrogel precursor solutions (1 mL) prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were respectively injected onto the surface of a membrane sheet (40×15 mm) and cured by ultraviolet irradiation;

[0087] Another PET film was bonded to the cured hydrogel (40×15 mm) with CA adhesive, and uniaxial tension was applied at a constant loading rate of 1 mm / min using an Instron machine (Instron-5543 equipped with a 1 kN sensor). No peeling occurred in Examples 1 to 3 and Comparative Examples 1 to 2.

[0088] 3. Antibacterial test

[0089] Prepare a culture medium for Staphylococcus aureus; spread 10 -8 of Staphylococcus aureus stock solution;

[0090] The hydrogels for preparing traumatic wound sealants prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were processed into discs with a diameter of 6 mm and a thickness of 2 mm respectively; the discs were soaked in alcohol and sterilized by ultraviolet light, then dried by an alcohol lamp and placed in a culture medium, and the culture medium was cultured in a constant temperature incubator at 37° C. for 24 h, and the size of the inhibition ring was tested, and the diameter of the inhibition ring was taken as the antibacterial property. The results are shown in Table 1;

[0091] Table 1 Explosion pressure and antibacterial property of hydrogels prepared in Examples 1 to 3 and Comparative Examples 1 to 2

[0092] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Burst pressure / mmHg 203 198 205 174 42 Antibacterial property / mm 12.6 13.1 12.7 0 12.5

[0093] It can be found from Table 1 that the hydrogel material for preparing a traumatic wound sealant provided by the present invention has a burst pressure higher than 150 mmHg (human arterial blood pressure), and does not peel off after a peeling test, has good adhesion, and can be well used for adhesion and sealing of traumatic wounds in vivo, and the hydrogel material for preparing a traumatic wound sealant has antibacterial properties.

[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a hydrogel material for preparing a traumatic wound sealant, characterized in that: The following steps are involved: 1) mixing gelatin, a first buffer solution and methacrylic anhydride, and performing an esterification reaction to obtain methacrylated gelatin; 2) mixing a soluble starch aqueous solution, a silver nitrate aqueous solution, a β-D glucose aqueous solution and the methacrylylated gelatin to obtain methacrylylated gelatin-nanosilver; 3) mixing the methacrylated gelatin-nanosilver, silanized hyaluronic acid, LAP photoinitiator and a second buffer solution to obtain a hydrogel precursor solution; The hydrogel precursor solution is photocured under ultraviolet light irradiation conditions to obtain a hydrogel material for preparing a traumatic wound sealant.

2. The preparation method according to claim 1, characterized in that: Step 1) The first buffer solution is a PBS solution; the usage ratio of gelatin to the first buffer solution is 1g:5-12mL; the usage ratio of gelatin to methacrylic anhydride is 1g:0.1-0.3mL.

3. The preparation method according to claim 1, characterized in that: Step 1) The temperature of the esterification reaction is 40-60°C and the time is 2-5 hours.

4. The preparation method according to claim 1, characterized in that: Step 2) The concentration of the soluble starch is 5-9 g / L; the volume ratio of the soluble starch aqueous solution to the silver nitrate aqueous solution is 50-300:0.05-0.

5.

5. The preparation method according to claim 1 or 4, characterized in that: Step 2) The concentration of the silver nitrate aqueous solution is 0.09-0.12 mol / L; the concentration of the β-D glucose aqueous solution is 0.09-0.12 mol / L; the volume ratio of the silver nitrate aqueous solution to the β-D glucose aqueous solution is 0.8-1.2:1; the mass ratio of the soluble starch aqueous solution to the methacryloyl gelatin is 0.5-3:1-4.

6. The preparation method according to claim 1, characterized in that: Step 3) In the hydrogel precursor solution, the concentration of methacrylated gelatin-nanosilver is 5-10wt%, the concentration of silanized hyaluronic acid is 1-2.5wt%, and the concentration of LAP photoinitiator is 0.1-0.5wt%.

7. The preparation method according to claim 1 or 6, characterized in that: Step 3) The second buffer solution is a PBS solution; the wavelength of the ultraviolet light is 300-405 nm, and the power is 25-40 mW / cm 2 , the light curing time is 5 to 15 seconds.

8. A hydrogel material for preparing a traumatic wound sealant obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the hydrogel material for preparing a traumatic wound sealant according to claim 8 in preparing a traumatic wound sealant.