PVDF / WH composite piezoelectric film and preparation method thereof
The piezoelectric film was prepared by combining PVDF with annealed white phosphate calcium stone, which solved the problem of poor piezoelectricity of bionic periosteum, achieved excellent piezoelectric properties and antibacterial effects, and promoted the bone healing process.
Patent Information
- Application Number
- CN202410967527.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The existing bionic periosteum has poor piezoelectric properties, which is difficult to effectively promote bone healing, and the osteogenic materials are poor in compatibility when they are combined with piezoelectric materials, affecting piezoelectric properties.
PVDF and annealed white phosphate (WH) were used to prepare piezoelectric films. Through annealing treatment, dispersion, mixing, drying, corona polarization and other steps, PVDF/WH composite piezoelectric with excellent piezoelectric properties was prepared. film.
It improves the piezoelectric properties of the composite film, can generate endogenous electrical stimulation under mechanical stress, promotes bone tissue regeneration, and has good antibacterial properties, significantly improving bone repair efficiency and clinical application prospects.
Smart Images

Figure CN118903540A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomedical materials, and in particular relates to a PVDF / WH composite piezoelectric film and a preparation method thereof. Background Art
[0002] Bone defects and nonunion are the most common and serious complications after fractures, with an incidence of 5-10%, which is challenging in clinical application. There is electrical potential in natural human bones. Electrical stimulation, as one of the most commonly used physical therapies, has been proven to promote bone healing. However, the inconvenience and uncertainty of using in vitro electrical stimulation increase the difficulty of clinical application.
[0003] Piezoelectric materials can generate electrical signals in response to mechanical stress, which serve as endogenous electrical stimuli to stimulate signal pathways and promote tissue regeneration in damaged areas. However, the simple application of piezoelectric materials cannot provide the calcium, phosphorus and other ions required for osteogenesis, and usually requires the addition of osteogenic materials such as hydroxyapatite. When osteogenesis materials and piezoelectric materials are combined to prepare bionic periosteum, the compatibility of the two must also be considered to ensure the piezoelectricity of the resulting bionic periosteum. Summary of the invention
[0004] The purpose of the present invention is to overcome the above technical deficiencies, provide a PVDF / WH composite piezoelectric film and a preparation method thereof, and solve the technical problem of poor piezoelectricity of bionic periosteum in the prior art.
[0005] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a method for preparing a PVDF / WH composite piezoelectric film, comprising the following steps: S1, annealing white patenite A to obtain white patenite B with piezoelectricity; S2, dispersing white patenite B in a first solvent to obtain a WH dispersion, and then mixing it with a PVDF solution to obtain a mixed solution; S3, spreading the mixed solution on a substrate, drying it, heating it, and then cooling it to room temperature to obtain a PVDF / WH composite film; S4, corona polarization treating the PVDF / WH composite film to obtain a PVDF / WH composite piezoelectric film.
[0006] In a second aspect, the present invention provides a PVDF / WH composite piezoelectric film prepared by the above method.
[0007] Compared with the prior art, the beneficial effects of the present invention include: The present invention incorporates annealed white patite into PVDF to prepare a flexible PVDF / WH composite piezoelectric film. The annealed white patite gives the material the ability to repair bones, while effectively improving the low piezoelectricity of PVDF. Therefore, the composite piezoelectric film prepared by the present invention has excellent piezoelectricity, can generate endogenous electrical stimulation after being subjected to mechanical stress, and then effectively stimulates bone tissue regeneration, inhibits bacterial infection during the repair process, and greatly improves the efficiency of bone repair. The composite piezoelectric film preparation method of the present invention is simple, the obtained composite piezoelectric film has strong wound adaptability, and has good clinical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 1 are SEM images of WH particles prepared by the present invention before and after annealing, wherein (a) is WH (before annealing) and (b) is WH-650 (after annealing); Figure 2 It is the XRD test diagram of WH and WH-650 of the present invention compared with the standard card; Figure 3 FTIR detection diagrams of the PVDF film obtained in Comparative Example 2 of the present invention and the PVDF / WH composite piezoelectric film obtained in Example 1-2; Figure 4 is the water contact angle of the PVDF film obtained in Comparative Example 2 of the present invention and the PVDF / WH composite piezoelectric film obtained in Examples 1-2; Figure 5 is the piezoelectric coefficient d of the films obtained in the embodiments of the present invention and the comparative examples. 33 Comparison; wherein (a) is the PVDF film obtained in Comparative Examples 1-3, (b) is Comparative Example 2 and Examples 1-2, (c) is Comparative Example 2 and Comparative Example 5, and (d) is Comparative Example 6 and Example 1; Figure 6 It is the voltage output of the PVDF film obtained in Comparative Example 2 of the present invention and the PVDF / WH composite piezoelectric film obtained in Examples 1-2. DETAILED DESCRIPTION
[0009] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0010] In view of the problem that the piezoelectricity of the obtained bionic periosteum may be poor due to the incompatibility of the two when osteogenic materials and piezoelectric materials are composited to prepare bionic periosteum, the present invention provides a PVDF / WH composite piezoelectric film and a preparation method thereof, with PVDF and white calcium apatite as the main raw materials, wherein PVDF is a piezoelectric polymer with excellent flexibility and ductility, and exhibits good biocompatibility. The metabolic process of bacteria has various cell-to-cell interaction signals, which act between cells to complete the life vitality process. The exogenous electric field generated by PVDF after stress may cause the destruction of the charge distribution of the cell membrane, thereby applying voltage stress to the bacterial organism and inhibiting bacterial growth; compared with the commonly used bone repair material hydroxyapatite, WH has better osteogenic repair ability. After annealing, WH has piezoelectricity, which can promote cell osteogenic differentiation while cooperating with PVDF to enhance the ability of bone repair; after testing, the composite piezoelectric film prepared by the present invention has excellent piezoelectricity and can be used as a bionic periosteum.
[0011] In a first aspect, the present invention provides a method for preparing a PVDF / WH composite piezoelectric film, comprising the following steps: S1, annealing the white phosphate A to obtain white phosphate B with piezoelectricity; S2, dispersing white patrite B in the first solvent to obtain a WH dispersion, and then mixing it with the PVDF solution to obtain a mixed solution; S3, spreading the mixed solution on a substrate, drying it, heating it, and then cooling it to room temperature to obtain a PVDF / WH composite film; S4, the PVDF / WH composite film is subjected to corona poling treatment to obtain a PVDF / WH composite piezoelectric film.
[0012] Preferably, the preparation steps of white phosphate calcium stone A specifically include: dissolving calcium hydroxide and magnesium hydroxide in deionized water, keeping warm at 95-100° C. for 0.4-0.6 h, then dropping a phosphoric acid solution, keeping the pH value of the reaction system at 4.5-5.5, reacting at 95-100° C. for 9-11 h, and after the reaction is completed, aging at room temperature for 12-14 h, and then washing and drying to obtain white phosphate calcium stone A.
[0013] Whitlockite (WH:Ca 18 Mg2(HPO4)2(PO4) 12) is one of the main components of natural bone tissue, accounting for about 20% of bone mineral, second only to hydroxyapatite. The non-centrosymmetric structure makes WH have piezoelectric properties, which can generate bioelectric signals similar to natural tissue to effectively promote bone tissue regeneration. Compared with the common bone repair material hydroxyapatite, WH has a stronger ability to promote stem cell differentiation in vitro and induce bone regeneration. WH can release Mg with repair function 2+ , which is beneficial to cell proliferation, adhesion and migration, promotes angiogenesis, and effectively induces osteogenesis. However, the synthesis of WH is difficult, there are many intermediates, and failure to strictly control the synthesis conditions will affect the crystallinity of the product. The present invention can produce white calcium phosphate with good crystallinity.
[0014] Further preferably, the molar ratio of calcium hydroxide, magnesium hydroxide and phosphoric acid added in the reaction is 0.37:0.13:0.5.
[0015] Preferably, in step S1, annealing is performed at 600-700°C for 2.5-3.5h; specifically, the annealing temperature can be selected from 600°C, 620°C, 640°C, 650°C, 660°C, 680°C, 700°C, etc., and the time can be selected from 2.5h, 2.8h, 3h, 3.2h, 3.5h, etc.
[0016] Preferably, in step S2, the mass ratio of white patrite B and PVDF in the mixed solution is (50-150) mg:1g, specifically selected from 50 mg:1g, 60 mg:1g, 80 mg:1g, 90 mg:1g, 100 mg:1g, 120 mg:1g, 150 mg:1g, etc.
[0017] Preferably, in step S2, the concentration of the WH dispersion is 50-150 mg / mL, specifically selected from 50 mg / mL, 80 mg / mL, 100 mg / mL, 120 mg / mL, 150 mg / mL, etc.
[0018] Preferably, in step S2, the concentration of the PVDF solution is 0.05-0.15 g / mL, specifically selected from 0.05 g / mL, 0.08 g / mL, 0.1 g / mL, 0.12 g / mL, 0.15 g / mL, etc.; the PVDF solution is obtained by dissolving PVDF in the second solvent and stirring for 5-6 hours; the first solvent and the second solvent both include DMF.
[0019] Preferably, in step S3, drying is performed at 45-55° C. for 12-16 hours.
[0020] Preferably, in step S3, the heating treatment is maintained at 120-140°C for 0.8-1.2h. Specifically, the temperature can be selected from 120°C, 125°C, 130°C, 135°C, 140°C, etc., and the time can be selected from 0.8h, 0.9h, 1h, 1.1h, 1.2h, etc.
[0021] Preferably, in step S3, the substrate is a smooth quartz plate.
[0022] Preferably, in step S4, the conditions for the corona poling treatment are: a voltage of 20 to 28 kV and a time of 25 to 35 min. Specifically, the voltage can be selected from 20 kV, 22 kV, 24 kV, 25 kV, 28 kV, etc., and the time can be selected from 25 min, 30 min, 35 min, etc. A polarization voltage that is too high or a time that is too long will lead to over-polarization of the film, and a time that is too short will lead to insufficient polarization of the film, and the optimal piezoelectric performance cannot be obtained.
[0023] In a second aspect, the present invention provides a PVDF / WH composite piezoelectric film prepared by the above method, wherein the thickness of the film is 0.06 to 0.15 mm. In the present invention, the annealed WH is compounded into the PVDF membrane by a simple casting method, and its main mechanism and advantages are: (1) Piezoelectricity: The present invention utilizes the piezoelectricity of annealed white calcium apatite and combines it with PVDF, which has relatively weak piezoelectricity, to synergistically produce excellent piezoelectric performance; (2) Antibacterial property: The PVDF / WH composite piezoelectric film prepared by the present invention has excellent piezoelectricity. When squeezed by muscle, it can deform and generate surface charge, thereby providing the physiological electrical microenvironment required for the bone defect, affecting the life activities of bacteria, and achieving antibacterial effect without relying on the direct contact mechanism of antibacterial nanoparticles; (3) The prepared composite film material is evenly dispersed, has excellent mechanical properties, is wound adaptable, and has broad application prospects in clinical practice.
[0024] The present invention is further described in detail below through specific examples and comparative examples; to avoid redundancy, some raw materials are described here, and other reagents not separately described are all conventional products that can be obtained commercially.
[0025] Preparation of WH: First, Ca(OH)2 and Mg(OH)2 were dissolved in deionized water and maintained at 100°C for 0.5 h. Then, H3PO4 solution (100 mL, 0.5 M) was added dropwise at a rate of 12.5 mL / min. The pH value of the system was kept at 5. The reaction was carried out at 100°C for 10 h. The molar ratio of Ca(OH)2, Mg(OH)2 and H3PO4 was controlled to be 0.37:0.13:0.5. After heating, the particles were aged at room temperature for 14 h, washed three times with deionized water and anhydrous ethanol, and dried overnight at 70°C to obtain WH particles.
[0026] Preparation of WH-650 (white calcium phosphate with piezoelectricity): WH was annealed in a muffle furnace at 650°C for 3 h to obtain WH-650 with piezoelectricity.
[0027] Comparative Example 1 A PVDF piezoelectric film, the preparation method of which comprises the following steps: Weigh 1 g of PVDF powder and add it to 10 ml of DMF (N,N-dimethylformamide), stir magnetically for 6 h until fully dissolved to obtain a PVDF solution. Spread the evenly stirred PVDF solution on a smooth quartz plate, place it horizontally in an oven, and dry it at 50°C overnight. Finally, set the oven temperature to 110°C, keep it for 1 hour, and then naturally cool it down to room temperature for annealing, and peel the PVDF film off the quartz plate.
[0028] The prepared PVDF film was cut into 5 cm × 5 cm squares, placed on a corona polarization metal plate, and subjected to corona polarization treatment at 24 kV for 30 min to obtain a PVDF piezoelectric film.
[0029] Comparative Example 2 A PVDF piezoelectric film, the preparation method of which is different from that of Comparative Example 1 only in that the oven temperature is set to 120° C., and the other steps and conditions are the same as those of Comparative Example 1.
[0030] Comparative Example 3 A PVDF piezoelectric film, the preparation method of which is different from that of Comparative Example 1 only in that the oven temperature is set to 130° C., and the other steps and conditions are the same as those of Comparative Example 1.
[0031] Example 1 A method for preparing a PVDF / WH composite piezoelectric film comprises the following steps: First, WH-650 was evenly dispersed in DMF using a homogenizer at 8000 rpm to prepare a 100 mg / mL WH dispersion. 1 g of PVDF powder was weighed and added to 8 ml of DMF (N,N-dimethylformamide), and magnetically stirred for 6 h until fully dissolved to obtain a PVDF solution.
[0032] Then, 1 mL of WH dispersion was added to the PVDF solution and stirred to mix the dispersion evenly. The evenly stirred mixed solution was spread on a smooth quartz plate, placed horizontally in an oven, and dried at 50°C for 14 hours. Finally, the oven temperature was set to 120°C, maintained for 1 hour, and then rapidly cooled and annealed to room temperature, and the composite film was peeled off the quartz plate to obtain a composite film with a WH content of 10 wt% of the PVDF content.
[0033] The composite film prepared above was cut into 5 cm × 5 cm squares and placed on a corona polarized metal plate. The corona polarization conditions were 24 kV and 30 min. The film after polarization had piezoelectricity, namely, PVDF / WH composite piezoelectric film, named PVDF / WH-10. The thickness of the composite piezoelectric film was about 0.08 mm.
[0034] Example 2 A method for preparing a PVDF / WH composite piezoelectric film comprises the following steps: First, WH-650 was evenly dispersed in DMF using a homogenizer at 8000 rpm to prepare a 100 mg / mL WH dispersion. 1 g of PVDF powder was weighed and added to 8 ml of DMF (N,N-dimethylformamide), and magnetically stirred for 6 h until fully dissolved to obtain a PVDF solution.
[0035] Then, 1.5 mL of WH dispersion was added to the PVDF solution and stirred for several hours to mix the dispersion evenly. The evenly stirred mixed solution was spread on a smooth quartz plate, placed horizontally in an oven, and dried at 50°C for 14 hours. Finally, the oven temperature was set to 120°C, maintained for 1 hour, and then rapidly cooled and annealed to room temperature, and the composite film was peeled off the quartz plate to obtain a composite film with a WH content of 15 wt% of the PVDF content.
[0036] The composite film prepared above was cut into 5 cm × 5 cm squares, placed on a corona polarization metal plate, and subjected to corona polarization treatment. The corona polarization treatment conditions were the same as those in Example 1. The obtained PVDF / WH composite piezoelectric film was named PVDF / WH-15, and the thickness of the composite piezoelectric film was about 0.08 mm.
[0037] Comparative Example 4 A method for preparing a PVDF / WH composite piezoelectric film, which is different from Example 1 in that 2 mL of WH dispersion is added to the PVDF solution, and the other steps and conditions are the same as those in Example 1. The obtained PVDF / WH composite piezoelectric film is named PVDF / WH-20.
[0038] Examples 1-2 and Comparative Example 4 explore the effect of WH-650 on the performance of PVDF film by changing the amount of WH-650 added, but excessive WH addition (20%) will cause the film to curl and not form, affecting subsequent experimental tests and material effects. Therefore, the maximum amount of WH in the present invention is set to 15 wt% of the PVDF content.
[0039] Comparative Example 5 The only difference from Example 1 is that the annealing process of WH is removed, that is, WH is used to replace WH-650. The other steps and conditions are the same as those in Example 1 to obtain a PVDF / WH composite film.
[0040] Comparative Example 6 The only difference from Example 1 is that PCL is used to replace PVDF, and the other steps and conditions are the same as those in Example 1 to obtain a PCL / WH-10 composite film.
[0041] Performance Testing 1. Scanning electron microscope Figure 1 The scanning electron microscope images of WH particles (a) and WH-650 particles (b) prepared in the present invention show that the WH particles synthesized in the present invention have a regular and uniform prism shape, and the shape of the WH-650 particles changes from prism to sphere after high-temperature annealing.
[0042] 2. XRD detection XRD was used to analyze the material structure and crystal phase composition of WH and WH-650. The results are as follows: Figure 2 shown.
[0043] See also Figure 2 By comparing with the standard card of WH, the main peak positions of the synthesized WH are located at 34.64°, 28.02° and 31.28°, and the corresponding crystal planes are (2 2 0), (0 2 10) and (2 1 4), respectively. The results correspond to the WH crystal form of PDF#70-2064, proving that the present invention synthesizes a pure WH phase. The main peaks of the WH-650 curves before annealing and after annealing remain consistent, indicating that heat treatment has no effect on the crystal phase of the particles.
[0044] 3. FTIR detection The PVDF / WH composite piezoelectric films (PVDF / WH-10 and PVDF / WH-15) obtained in Examples 1-2 and the PVDF film obtained in Comparative Example 2 were subjected to FTIR detection. The results are as follows: Figure 3 shown.
[0045] Figure 3 The results showed that 924 cm -1 The peak at is HPO4 2- The characteristic peaks of the group belong to the characteristic peaks of WH, which proves that WH is successfully compounded into PVDF film. PVDF has only β phase as the electroactive phase, and the typical characteristic peaks of β phase are 1280, 840 and 510 cm -1 Characteristic peaks can be observed everywhere, proving that the product of the present invention has good piezoelectricity.
[0046] 4. Water contact angle test The hydrophilicity of the PVDF / WH composite piezoelectric films (PVDF / WH-10 and PVDF / WH-15) obtained in Examples 1-2 and the PVDF film obtained in Comparative Example 2 was investigated by the static contact angle method. The results are as follows: Figure 4 shown.
[0047] Depend on Figure 4 It can be seen that the water contact angle of the product of the present invention increases slightly with the addition amount of WH. The water contact angle of the PVDF film prepared in Comparative Example 2 is about 72.8°, the water contact angle of Example 1 is about 75.6°, and that of Example 2 is about 81.8°. All three are within the hydrophilic range (<90°), which is conducive to cell adhesion and proliferation, and provides a good environment for osteogenic differentiation.
[0048] 5.d 33 Detection At room temperature, using quasi-static 33 The piezoelectric coefficient d of the PVDF and PVDF / WH piezoelectric films of different embodiments and comparative examples is measured by a tester. 33 , the results are as follows Figure 5 shown.
[0049] like Figure 5 As shown in (a), comparative examples 1-3 explore the effect of PVDF annealing temperature on the piezoelectric properties of PVDF. The piezoelectric coefficient d33 test shows that when the annealing temperature is 120°C, the piezoelectric performance of PVDF is the best, reaching 15.7pC / N. Therefore, the preferred annealing temperature of the present invention is 120°C.
[0050] like Figure 5 As shown in (b), after adding 10 wt% WH, the d 33 increased to 19.45 pC / N, and after further increasing the compounding amount of WH (Example 2), d 33On the contrary, it decreases, indicating that Example 1 has the best piezoelectric performance.
[0051] like Figure 5 As shown in (c), compared with Comparative Example 2 and Comparative Example 5, there is no obvious difference in the piezoelectric coefficient of the PVDF / WH composite film obtained in Comparative Example 5 and the PVDF film of Comparative Example 2, indicating that the unannealed WH particles are not electrically active. Therefore, the present invention prefers the annealed WH-650.
[0052] like Figure 5 As shown in (d), the piezoelectric coefficient of the PCL / WH-10 composite film obtained by compounding PCL and WH-650 in Comparative Example 6 is 7.6 pC / N, which is even worse than the piezoelectric performance of the PVDF film alone. The piezoelectric coefficient of the PVDF / WH composite piezoelectric film (PVDF / WH-10) obtained in Example 1 is 19.45 pC / N, which has more excellent piezoelectric performance. This shows that the present invention uses PVDF and WH-650 to compound, which have good compatibility and synergistically produce excellent piezoelectric performance.
[0053] 6. Electrical performance test An electrochemical workstation was used to detect the voltage output performance of the PVDF / WH composite piezoelectric film. Before testing the piezoelectric output performance, the film needed to be packaged. The upper and lower layers were made of copper foil (Cu) as electrodes, and the middle layer was the prepared piezoelectric film. Wires were used to connect to the copper electrodes of the upper and lower layers, and polyethylene terephthalate (PET) film was used to package the device. A fixed mechanical stress of 5 N was applied to the three groups of piezoelectric films in Comparative Example 2 and Examples 1-2 at a frequency of 0.5 Hz to test the piezoelectric output effect of the film. The results are shown in Figure 2. Figure 6 shown.
[0054] See also Figure 6 With the increase of the WH-650 compounding amount, the voltage output of the film shows a trend of first increasing and then decreasing. The PVDF / WH-10 prepared in Example 1 has the highest voltage output of about 1.48 V, indicating that it has the best electrical properties.
[0055] In summary, the present invention utilizes white patrite combined with PVDF to significantly enhance the piezoelectricity of the resulting film, which can provide a good electrical microenvironment for the bone defect site, thereby promoting bone repair and providing a certain antibacterial property.
[0056] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a PVDF / WH composite piezoelectric film, characterized in that: The following steps are involved: S1, annealing the white phosphate A to obtain white phosphate B with piezoelectricity; S2, dispersing white patrite B in the first solvent to obtain a WH dispersion, and then mixing it with the PVDF solution to obtain a mixed solution; S3, spreading the mixed solution on a substrate, drying it, heating it, and then cooling it to room temperature to obtain a PVDF / WH composite film; S4, the PVDF / WH composite film is subjected to corona poling treatment to obtain a PVDF / WH composite piezoelectric film.
2. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: The preparation steps of the white phosphate A specifically include: dissolving calcium hydroxide and magnesium hydroxide in deionized water, keeping the temperature at 95-100° C. for 0.4-0.6 h, then dropping a phosphoric acid solution, keeping the pH value of the reaction system at 4.5-5.5, reacting at 95-100° C. for 9-11 h, and after the reaction is completed, aging at room temperature for 12-14 h, and then washing and drying to obtain the white phosphate A.
3. The method for preparing the PVDF / WH composite piezoelectric film according to claim 2, characterized in that: The molar ratio of the calcium hydroxide, magnesium hydroxide and phosphoric acid is 0.37:0.13:0.
5.
4. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: In step S1, the annealing treatment is performed at 600-700°C for 2.5-3.5h.
5. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: In step S2, the mass ratio of white patrite B to PVDF in the mixed solution is (50-150) mg:1 g.
6. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: In step S2, the concentration of the WH dispersion is 50-150 mg / mL; The concentration of the PVDF solution is 0.05-0.15 g / mL; The PVDF solution is obtained by dissolving PVDF in a second solvent and stirring for 5 to 6 hours; the first solvent and the second solvent both include DMF.
7. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: In step S3, the drying is carried out at 45-55° C. for 12-16 hours; The substrate is a smooth quartz plate.
8. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: In step S3, the heating treatment is maintained at 120-140°C for 0.8-1.2h.
9. The method for preparing the PVDF / WH composite piezoelectric film according to claim 1, characterized in that: In step S4, the conditions of the corona poling treatment are: voltage of 20-28 kV, and time of 25-35 min.