Atlantoaxial PEEK interbody fusion cage tooth surface composite coating
By forming a transition layer on the PEEK surface and spraying a nano-hydroxyapatite coating, the problem of low binding strength between hydroxyapatite and PEEK is solved, the long-term biocompatibility and mechanical stability of the material are achieved, and bone tissue growth is promoted. .
Patent Information
- Application Number
- CN202411154439.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-22
AI Technical Summary
There is a large difference in chemical and physical properties between the inorganic material hydroxyapatite and the polymer material PEEK, resulting in low binding strength of the two.
Using transition layer technology, epoxidized hydroxyapatite and phosphorylated PEEK are grafted through chemical bonds to prepare transition layer slurry, and a nano-hydroxyapatite coating is formed on the PEEK surface through plasma spraying technology to adjust the thermal expansion coefficient and elasticity. Modulus gradient to improve binding strength.
It significantly improves the binding strength between hydroxyapatite and PEEK, reduces the risk of coating shedding, enhances the biocompatibility and mechanical stability of the material, and promotes cell attachment and bone tissue growth.
Smart Images

Figure CN118903556A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical materials, and in particular to a composite coating on the tooth surface of an atlantoaxial PEEK intervertebral fusion device. Background Art
[0002] Lumbar degenerative diseases are very common in orthopedic clinics, including lumbar disc herniation, lumbar degenerative slippage, etc., which may cause low back pain and nerve compression symptoms, seriously affecting the patient's quality of life. The occurrence of atlantoaxial disease causes most patients to suffer from atlantoaxial instability, which further leads to spinal cord compression and nerve damage. Surgery is often required to completely relieve the compression and restore the physiological curvature of the lumbar spine. At present, the clinical treatment of atlantoaxial fixation and fusion is fixed by simple bone grafting and fusion, and the bone graft material is mainly autologous iliac bone. The simple bone grafting fixation method makes the fusion site lack stress load, which is prone to complications such as collapse and false joint formation. Combined with the application of conventional PEEK fusion devices in spinal fusion devices, our company has designed a PEEK intervertebral fusion device with surface coating modification for atlantoaxial combined with many years of actual surgical operations of clinicians.
[0003] Polyetheretherketone (PEEK) resin is a synthetic semi-crystalline polymer with an elastic modulus similar to that of cortical bone. It also has the advantages of good biocompatibility, radiotransmittance, and no artifacts in magnetic resonance scanning. It is valued by the medical device industry, especially the implantable medical industry. However, since PEEK is a hydrophobic and bioinert material, this low surface energy can limit cell adhesion, and its bone conduction and bone integration capabilities are limited, resulting in the inability of the material to promote the attachment and proliferation of osteoblasts after implantation in the body. In order to obtain a PEEK implant with good bone integration performance, its surface needs to be modified. Common modification methods to improve bone integration performance include surface coating technology and surface treatment technology. Surface coating is a commonly used material surface modification technology that can not only improve the biological properties of PEEK, but also preserve its original mechanical properties. Among them, bioactive materials such as titanium (Ti) and hydroxyapatite (HA) are coated on the PEEK surface to improve its bone integration performance. Titanium has excellent mechanical and biocompatibility and can promote bone growth. The growth and diffusion of cells on the surface of titanium-coated PEEK are more active, but titanium coatings can cause artifacts in medical imaging and affect the visualization of the interface between bone and implant. Hydroxyapatite is the main component of human bones and is superior to titanium in terms of biocompatibility. However, the chemical and physical properties of the inorganic material hydroxyapatite and the polymer material PEEK are quite different, resulting in low bonding strength between the two and easy coating shedding. Summary of the invention
[0004] The purpose of the present invention is to provide a composite coating on the tooth surface of an atlantoaxial PEEK interbody fusion device to solve the following technical problems: The chemical and physical properties between the inorganic material hydroxyapatite and the polymer material PEEK are quite different, resulting in low bonding strength between the two.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A composite coating for tooth surfaces of an atlantoaxial PEEK intervertebral fusion device, comprising a transition layer coated on the tooth surfaces of the atlantoaxial PEEK intervertebral fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method of the transition layer comprises the following steps: S1: Add epoxidized hydroxyapatite and sulfolane into a reaction kettle and disperse them evenly, and control the temperature at 210-220° C. to obtain solution A; S2: Phosphorylated PEEK and sulfolane are added into a reactor, heated and stirred to dissolve, and solution A is added under heat preservation conditions to disperse evenly to obtain a transition layer slurry; S3: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature, and heat treating to obtain the transition layer; The preparation method of epoxidized hydroxyapatite comprises the following steps: Add anhydrous ethanol and deionized water into a reaction kettle and disperse them evenly, adjust the pH to 4-5, add γ-glycidyloxypropyltriethoxysilane, stir at room temperature for 0.5-1h, add nano-hydroxyapatite, control the temperature at 60-65°C, keep warm and stir for 2-4h, filter, wash with water, and dry to obtain epoxidized hydroxyapatite; The preparation method of the phosphorylated PEEK comprises the following steps: A1: Add polyetheretherketone and concentrated sulfuric acid into a reaction kettle, control the temperature at 0-5°C, disperse until the solution becomes transparent, add chloromethyloctyl ether, keep warm and stir for 1-3 hours, add ice water to stop the reaction, filter, wash with water until neutral, wash with ethanol, and dry to obtain component 1; A2: Add component 1 and N-methylpyrrolidone into the reaction kettle and disperse them evenly, add triethyl phosphite, control the temperature at 110-120°C, keep the reaction warm for 12-18 hours, remove triethyl phosphite by vacuum distillation, wash with water, dry, add concentrated hydrochloric acid, heat and reflux for 9-15 hours, filter, wash with water, and dry to obtain phosphorylated PEEK.
[0006] As a further scheme of the present invention: the preparation method of the nano hydroxyapatite comprises the following steps: 0.5-2.5 mol / L calcium nitrate tetrahydrate [Ca(NO3)2·4H20] aqueous solution, 0.5-3 mol / L diammonium hydrogen phosphate [(NH4)2HPO4] aqueous solution and ammonium fluoride are used as raw materials, prepared according to a Ca:P:F molar ratio of 16.7:10:1, 10-30wt% ammonia water is used to adjust the pH to 9-10, the temperature is controlled at 60-90°C, the reaction is kept warm, filtered, aged for 24-48h, and dialyzed with deionized water to remove ammonia and salts to obtain nano hydroxyapatite.
[0007] As a further solution of the present invention: the epoxidized hydroxyapatite accounts for 30-50% of the total mass of the transition layer.
[0008] As a further solution of the present invention: the thickness of the transition layer is 15-125 um.
[0009] As a further solution of the present invention: the addition ratio of anhydrous ethanol, deionized water, γ-glycidyloxypropyltriethoxysilane and nano-hydroxyapatite is 45-90 mL: 5-10 mL: 2.5-5 mL: 1 g.
[0010] As a further embodiment of the present invention, the addition ratio of polyetheretherketone, concentrated sulfuric acid and chloromethyloctyl ether in A1 is 1 g: 50-75 mL: 8-15 mL.
[0011] As a further solution of the present invention: the addition ratio of component 1, N-methylpyrrolidone and triethyl phosphite in A2 is 1g: 20-40mL: 2-4mL. As a further solution of the present invention: the hydroxyapatite coating is prepared by using nano-hydroxyapatite as a raw material to form a suspension, and the suspension is obtained by plasma spraying technology.
[0012] As a further solution of the present invention: the plasma spraying technology specifically includes the following steps: B1: mixing nano-hydroxyapatite and distilled water to obtain a suspension, wherein the solid content of the suspension is 5-15%; B2: The suspension is sprayed using plasma spraying technology to obtain a hydroxyapatite coating.
[0013] As a further solution of the present invention: the specific spraying parameters during the plasma spraying process are: gas flow rate 150-180 L / min, arc current 180-230 A, and spraying distance 50-80 mm.
[0014] As a further solution of the present invention: the thickness of the hydroxyapatite coating is 45-75 um.
[0015] As a further solution of the present invention: the transition layer is applied on the surface of a PEEK component of the atlantoaxial PEEK intervertebral fusion device; the PEEK component is obtained by subjecting PEEK resin to surface sulfonation treatment.
[0016] As a further solution of the present invention, the specific steps of the sulfonation treatment are: immersing the PEEK component in concentrated sulfuric acid, controlling the temperature to 50-70°C, keeping the temperature under stirring for 6-9 hours, adding ice water for washing, and drying As a further solution of the present invention: the concentrated sulfuric acid in the sulfonation treatment is an 85-98wt% sulfuric acid aqueous solution, and the addition ratio of PEEK to concentrated sulfuric acid is 1g:8-12mL.
[0017] As a further solution of the present invention: the atlantoaxial PEEK intervertebral fusion device comprises a device body, a developing pin for intraoperative developing and positioning, and a composite coating; the device body is made of PEEK resin, and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; As a further solution of the present invention: the developing nail is made of titanium alloy or pure tantalum material, and is used for intraoperative and postoperative development.
[0018] As a further solution of the present invention: a bone grafting window for filling bone grafting material is reserved in the middle part of the atlantoaxial PEEK intervertebral fusion device, and a circumferential protrusion ring structure is designed in the middle of the bone grafting window to facilitate the fixation of the bone grafting material; and an instrument clamping groove is designed at the tail of the product to facilitate the adjustment of the position of the fusion device during surgery.
[0019] Beneficial effects of the present invention: (1) The present application prepares epoxidized hydroxyapatite based on the prepared nano-hydroxyapatite by modifying it with an epoxysilane coupling agent. The present application uses concentrated sulfuric acid as a solvent to perform a chloromethylation reaction on polyetheretherketone using chloromethyl octyl ether to obtain chloromethylated polyetheretherketone, i.e., component one; and uses component one and triethyl phosphite as raw materials, and through the Michaels-Arbuzov reaction, uses the phosphate group of triethyl phosphite to replace the chloride ions on the molecular chain of component one, and finally hydrolyzes it to obtain phosphorylated PEEK; the present application mixes epoxidized hydroxyapatite and phosphorylated PEEK with sulfolane, respectively, and blends them under high temperature conditions, the epoxy groups of epoxidized hydroxyapatite and the phosphoric acid groups of phosphorylated PEEK undergo a ring-opening reaction, and hydroxyapatite is grafted onto the PEEK molecular chain through chemical bonds to prepare a transition layer slurry, and the transition layer slurry is coated on the surface of the sulfonated PEEK component, and a heat treatment is performed to remove the sulfolane in the transition layer slurry, and the heat treatment effectively improves the mechanical properties of the coating.
[0020] The present application uses the prepared epoxidized hydroxyapatite and phosphorylated PEEK as raw materials to prepare a transition layer, which effectively regulates the problem that the thermal expansion coefficient and elastic modulus between the hydroxyapatite coating and the PEEK component are relatively different, and residual stress is generated between the prepared coating material and the substrate, resulting in low bonding strength between the two. The present application introduces a transition layer between the coating and the substrate, and controls its thermal expansion coefficient and elastic modulus between the thermal expansion coefficient and elastic modulus of the substrate and the coating, thereby achieving a gradient change in the thermal expansion coefficient and elastic modulus of the material, reducing the residual stress between the substrate and the coating, and improving the bonding strength between the coating and the substrate. The prepared material can be used in biological organisms for a long time.
[0021] (2) The present application uses concentrated sulfuric acid to corrode the PEEK component, forming a three-dimensional porous structure on the surface of the PEEK component, and also generates sulfonic acid groups on the surface and pores of the PEEK. The sulfonation treatment of PEEK by the present application not only increases the surface roughness of PEEK, improves hydrophilicity, and improves the bone integration performance of PEEK implants, but also improves the adhesion of cells and promotes the growth of soft and hard tissues into the implant material, generating more biological anchors to improve its stability. In addition, the present application coats the prepared transition layer slurry on the surface of the PEEK component after the sulfonation treatment to improve the bonding strength between the transition layer and PEEK.
[0022] (3) The present application uses calcium nitrate tetrahydrate [Ca(NO3)2·4H20] aqueous solution, diammonium hydrogen phosphate [(NH4)2HPO4] aqueous solution, and ammonium fluoride as raw materials to prepare nano-hydroxyapatite. The nano-hydroxyapatite prepared in the present application is doped with fluoride ions. Fluoride ions not only have an antibacterial effect, but also have a smaller radius than that of hydroxyl groups. The incorporation of fluoride ions reduces the crystal constant of hydroxyapatite, improves the crystal stability, and reduces the solubility of the coating in the human body.
[0023] (4) This application uses suspension ion spraying technology to mix the prepared hydroxyapatite with distilled water to prepare a suspension, and sprays the hydroxyapatite coating on the surface of the PEEK substrate with a transition layer attached. This application uses distilled water as a pore-forming agent. The prepared hydroxyapatite coating has a good porous structure, which is conducive to cell attachment, and the porous structure with a fully interconnected network is conducive to the ingrowth of osteoblasts. In addition to mechanical bonding, the bonding between the coating and the transition layer and the bonding between the coating particles can also produce micro-area metallurgical bonding and chemical bonding, and have a high bonding strength. This application uses suspension plasma spraying technology to prepare hydroxyapatite coatings, which does not require special vacuum or atmosphere, has high deposition efficiency and low preparation cost, and can effectively reduce material waste.
[0024] (5) The composite coating prepared in the present application covers the PEEK resin surface of the atlantoaxial PEEK interbody fusion device, and has initial stability and long-term mechanical stability. At the same time, the coating modification on the product surface can also provide the product with better fusion device fixation. The coating can guide the growth of new bone, provide a physiological scaffold for the formation of new bone, and closely integrate with bone tissue, greatly improving the bioactivity and biocompatibility of the PEEK surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention will be further described below in conjunction with the accompanying drawings.
[0026] Figure 1 This is a schematic diagram of the composite coating of the present application being applied to the tooth surface of the atlantoaxial PEEK interbody fusion device; Figure numerals: 1. Fusion device body; 2. Visualizing pin; 3. Composite coating. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0028] The preparation method of nano hydroxyapatite comprises the following steps: 2.5 mol / L calcium nitrate tetrahydrate [Ca(NO3)2·4H20] aqueous solution, 1.5 mol / L diammonium hydrogen phosphate [(NH4)2HPO4] aqueous solution and ammonium fluoride are used as raw materials and prepared according to a Ca:P:F molar ratio of 16.7:10:1. The pH value is adjusted to 10 with 30 wt% ammonia water, the temperature is controlled at 70°C, the reaction is kept warm, filtered, aged for 36 hours, and dialyzed with deionized water to remove ammonia and salts to obtain nano hydroxyapatite. Example 2
[0029] The preparation method of epoxidized hydroxyapatite comprises the following steps: 450 mL of anhydrous ethanol and 50 mL of deionized water were added to the reaction kettle and dispersed evenly, acetic acid buffer was added to adjust the pH to 4, 25 mL of γ-glycidyloxypropyltriethoxysilane was added, and stirred at room temperature for 0.5 h, 10 g of the nano-hydroxyapatite prepared in Example 1 was added and dispersed evenly, the temperature was controlled at 60° C., and the mixture was stirred at this temperature for 2 h, filtered, washed with water, and dried to obtain epoxidized hydroxyapatite; The preparation method of phosphorylated PEEK comprises the following steps: A1: Add 10g polyetheretherketone (PEEK 450PF powder produced by Victrex, UK) and 500mL 85wt% concentrated sulfuric acid into a reactor, control the temperature at 0℃, disperse until the solution becomes transparent, add 80mL chloromethyl octyl ether, keep warm and stir for 1h, add ice water to stop the reaction, filter, wash with water until neutral, wash with ethanol, and dry to obtain component 1; A2: 10 g of component 1 and 200 mL of N-methylpyrrolidone were added to the reactor and dispersed evenly. 20 mL of triethyl phosphite was added, the temperature was controlled at 110°C, and the reaction was kept warm for 12 hours. The triethyl phosphite was removed by vacuum distillation, washed with water, and dried. 36 wt% concentrated hydrochloric acid was added, and the mixture was heated under reflux for 9 hours. The mixture was filtered, washed with water, and dried to obtain phosphorylated PEEK. Example 3
[0030] The preparation method of epoxidized hydroxyapatite comprises the following steps: 630 mL of anhydrous ethanol and 70 mL of deionized water were added to the reaction kettle and dispersed evenly, acetic acid buffer was added to adjust the pH to 4, 35 mL of γ-glycidyloxypropyltriethoxysilane was added, and stirred at room temperature for 0.5 h, 10 g of the nano-hydroxyapatite prepared in Example 1 was added and dispersed evenly, the temperature was controlled at 65° C., and the mixture was stirred for 2 h at the temperature, filtered, washed with water, and dried to obtain epoxidized hydroxyapatite; The preparation method of phosphorylated PEEK comprises the following steps: A1: Add 10g polyetheretherketone (PEEK 450PF powder produced by Victrex, UK) and 650mL 85wt% concentrated sulfuric acid into a reactor, control the temperature at 0℃, disperse until the solution becomes transparent, add 120mL chloromethyl octyl ether, keep warm and stir for 1h, add ice water to stop the reaction, filter, wash with water until neutral, wash with ethanol, and dry to obtain component 1; A2: 10 g of component 1 and 300 mL of N-methylpyrrolidone were added to the reactor and dispersed evenly. 30 mL of triethyl phosphite was added, the temperature was controlled at 110°C, and the reaction was kept warm for 18 hours. The triethyl phosphite was removed by vacuum distillation, washed with water, and dried. 36 wt% concentrated hydrochloric acid was added, and the mixture was heated to reflux for 12 hours. The mixture was filtered, washed with water, and dried to obtain phosphorylated PEEK. Example 4
[0031] The preparation method of epoxidized hydroxyapatite comprises the following steps: 900 mL of anhydrous ethanol and 100 mL of deionized water were added to the reaction kettle and dispersed evenly, acetic acid buffer was added to adjust the pH to 4, 50 mL of γ-glycidyloxypropyltriethoxysilane was added, and stirred at room temperature for 1 h, 10 g of the nano-hydroxyapatite prepared in Example 1 was added and dispersed evenly, the temperature was controlled at 65° C., the mixture was stirred at this temperature for 4 h, filtered, washed with water, and dried to obtain epoxidized hydroxyapatite; The preparation method of phosphorylated PEEK comprises the following steps: A1: 10g polyetheretherketone (PEEK 450PF powder produced by Victrex, UK) and 750mL 85wt% concentrated sulfuric acid were added into a reactor, the temperature was controlled at 0℃, dispersed until the solution became transparent, 150mL chloromethyl octyl ether was added, the mixture was stirred at this temperature for 3h, ice water was added to stop the reaction, the mixture was filtered, washed with water until neutral, washed with ethanol, and dried to obtain component 1; A2: 10 g of component 1 and 400 mL of N-methylpyrrolidone were added to the reactor and dispersed evenly. 40 mL of triethyl phosphite was added. The temperature was controlled at 120°C and the reaction was kept warm for 18 hours. The triethyl phosphite was removed by vacuum distillation. The mixture was washed with water and dried. 36 wt% concentrated hydrochloric acid was added. The mixture was heated to reflux for 15 hours. The mixture was filtered, washed with water and dried to obtain phosphorylated PEEK. Example 5
[0032] See also Figure 1 The atlantoaxial PEEK intervertebral fusion device includes a device body 1, a developing pin 2 for intraoperative imaging positioning, and a composite coating 3; the device body is made of PEEK resin (PEEK 450PF powder produced by Victrex, UK), and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; The composite coating is a composite coating on the tooth surface of the atlantoaxial PEEK interbody fusion device, including a transition layer coated on the pre-treated tooth surface of the atlantoaxial PEEK interbody fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method for pre-treating the tooth surface of the atlantoaxial PEEK intervertebral fusion device comprises the following steps: The fusion device body 1 was immersed in 85wt% concentrated sulfuric acid at a solid-liquid ratio of 1g:10mL, the temperature was controlled at 60°C, the mixture was stirred and kept warm for 6 hours, ice water was added for washing, and the mixture was dried to obtain a pretreated atlantoaxial PEEK interbody fusion device; The preparation method of the transition layer comprises the following steps: S11: adding the epoxidized hydroxyapatite and sulfolane prepared in Example 2 into a reaction kettle and dispersing them evenly, controlling the temperature to 210° C., and obtaining a solution A; S12: adding the phosphorylated PEEK and sulfolane prepared in Example 2 into a reaction kettle and heating to 250° C., stirring and dissolving, adding solution A under heat preservation conditions and dispersing evenly to obtain a transition layer slurry; S13: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature at 270°C, sintering for 15 minutes, controlling the temperature at 170°C, and heat treating for 12 hours to obtain a transition layer with a thickness of 125 μm, wherein the epoxidized hydroxyapatite accounts for 30 wt%; The preparation method of hydroxyapatite coating comprises the following steps: S21: mixing the nano-hydroxyapatite prepared in Example 1 and distilled water to obtain a suspension, wherein the solid content of the suspension is 15%; S22: The suspension was sprayed using plasma spraying technology (gas flow rate 180 L / min, arc current 180 A, spraying distance 80 mm) to obtain a hydroxyapatite coating with a thickness of 75 um. Example 6
[0033] See also Figure 1 The atlantoaxial PEEK intervertebral fusion device includes a device body 1, a developing pin 2 for intraoperative imaging positioning, and a composite coating 3; the device body is made of PEEK resin (PEEK 450PF powder produced by Victrex, UK), and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; The composite coating is a composite coating on the tooth surface of the atlantoaxial PEEK interbody fusion device, including a transition layer coated on the pre-treated tooth surface of the atlantoaxial PEEK interbody fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method for pre-treating the tooth surface of the atlantoaxial PEEK intervertebral fusion device comprises the following steps: The fusion device body 1 was immersed in 85wt% concentrated sulfuric acid at a solid-liquid ratio of 1g:10mL, the temperature was controlled at 60°C, the mixture was stirred and kept warm for 6 hours, ice water was added for washing, and the mixture was dried to obtain a pretreated atlantoaxial PEEK interbody fusion device; The preparation method of the transition layer comprises the following steps: S11: adding the epoxidized hydroxyapatite and sulfolane prepared in Example 3 into a reaction kettle and dispersing them evenly, controlling the temperature to 210° C., to obtain a solution A; S12: adding the phosphorylated PEEK and sulfolane prepared in Example 3 into a reaction kettle and heating to 250° C., stirring and dissolving, adding solution A under heat preservation conditions and dispersing evenly to obtain a transition layer slurry; S13: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature at 270°C, sintering for 15 minutes, controlling the temperature at 170°C, and heat treating for 12 hours to obtain a transition layer with a thickness of 125 μm, wherein the epoxidized hydroxyapatite accounts for 30 wt%; The preparation method of hydroxyapatite coating comprises the following steps: S21: mixing the nano-hydroxyapatite prepared in Example 1 and distilled water to obtain a suspension, wherein the solid content of the suspension is 15%; S22: The suspension was sprayed using plasma spraying technology (gas flow rate 180 L / min, arc current 180 A, spraying distance 80 mm) to obtain a hydroxyapatite coating with a thickness of 75 um. Example 7
[0034] See also Figure 1 The atlantoaxial PEEK intervertebral fusion device includes a device body 1, a developing pin 2 for intraoperative imaging positioning, and a composite coating 3; the device body is made of PEEK resin (PEEK 450PF powder produced by Victrex, UK), and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; The composite coating is a composite coating on the tooth surface of the atlantoaxial PEEK interbody fusion device, including a transition layer coated on the pre-treated tooth surface of the atlantoaxial PEEK interbody fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method for pre-treating the tooth surface of the atlantoaxial PEEK intervertebral fusion device comprises the following steps: The fusion device body 1 was immersed in 85wt% concentrated sulfuric acid at a solid-liquid ratio of 1g:10mL, the temperature was controlled at 60°C, the mixture was stirred and kept warm for 6 hours, ice water was added for washing, and the mixture was dried to obtain a pretreated atlantoaxial PEEK interbody fusion device; The preparation method of the transition layer comprises the following steps: S11: adding the epoxidized hydroxyapatite and sulfolane prepared in Example 4 into a reaction kettle and dispersing them evenly, controlling the temperature to 210° C., and obtaining a solution A; S12: adding the phosphorylated PEEK and sulfolane prepared in Example 4 into a reaction kettle and heating to 250° C., stirring and dissolving, adding solution A under heat preservation conditions and dispersing evenly to obtain a transition layer slurry; S13: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature at 270°C, sintering for 15 minutes, controlling the temperature at 170°C, and heat treating for 12 hours to obtain a transition layer with a thickness of 125 μm, wherein the epoxidized hydroxyapatite accounts for 30 wt%; The preparation method of hydroxyapatite coating comprises the following steps: S21: mixing the nano-hydroxyapatite prepared in Example 1 and distilled water to obtain a suspension, wherein the solid content of the suspension is 15%; S22: The suspension was sprayed using plasma spraying technology (gas flow rate 180 L / min, arc current 180 A, spraying distance 80 mm) to obtain a hydroxyapatite coating with a thickness of 75 um.
[0035] Comparative Example 1 The preparation method of nano hydroxyapatite comprises the following steps: 2.5 mol / L calcium nitrate tetrahydrate [Ca(NO3)2·4H20] aqueous solution and 1.5 mol / L diammonium hydrogen phosphate [(NH4)2HPO4] aqueous solution were used as raw materials and prepared according to a Ca:P molar ratio of 16.7:10, and the pH was adjusted to 10 with 30 wt% ammonia water. The temperature was controlled at 70°C, the reaction was kept warm, filtered, aged for 36 hours, and dialyzed with deionized water to remove ammonia and salts to obtain nano hydroxyapatite.
[0036] Comparative Example 2 The preparation method of epoxidized hydroxyapatite comprises the following steps: 630 mL of anhydrous ethanol and 70 mL of deionized water were added to the reaction kettle and dispersed evenly, acetic acid buffer was added to adjust the pH to 4, 35 mL of γ-glycidyloxypropyltriethoxysilane was added, and stirred at room temperature for 0.5 h, 10 g of the nano-hydroxyapatite prepared in Comparative Example 1 was added and dispersed evenly, the temperature was controlled at 65° C., the mixture was stirred at this temperature for 2 h, filtered, washed with water, and dried to obtain epoxidized hydroxyapatite; The preparation method of phosphorylated PEEK comprises the following steps: A1: Add 10g polyetheretherketone (PEEK 450PF powder produced by Victrex, UK) and 650mL 85wt% concentrated sulfuric acid into a reactor, control the temperature at 0℃, disperse until the solution becomes transparent, add 120mL chloromethyl octyl ether, keep warm and stir for 1h, add ice water to stop the reaction, filter, wash with water until neutral, wash with ethanol, and dry to obtain component 1; A2: 10 g of component 1 and 300 mL of N-methylpyrrolidone were added to the reactor and dispersed evenly. 30 mL of triethyl phosphite was added, the temperature was controlled at 110°C, and the reaction was kept warm for 18 hours. The triethyl phosphite was removed by vacuum distillation, washed with water, and dried. 36 wt% concentrated hydrochloric acid was added, and the mixture was heated to reflux for 12 hours. The mixture was filtered, washed with water, and dried to obtain phosphorylated PEEK.
[0037] Comparative Example 3 See also Figure 1 The atlantoaxial PEEK intervertebral fusion device includes a device body 1, a developing pin 2 for intraoperative imaging positioning, and a composite coating 3; the device body is made of PEEK resin (PEEK 450PF powder produced by Victrex, UK), and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; The composite coating is a composite coating on the tooth surface of the atlantoaxial PEEK interbody fusion device, including a transition layer coated on the pre-treated tooth surface of the atlantoaxial PEEK interbody fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method for pre-treating the tooth surface of the atlantoaxial PEEK intervertebral fusion device comprises the following steps: The fusion device body 1 was immersed in 85wt% concentrated sulfuric acid at a solid-liquid ratio of 1g:10mL, the temperature was controlled at 60°C, the mixture was stirred and kept warm for 6 hours, ice water was added for washing, and the mixture was dried to obtain a pretreated atlantoaxial PEEK interbody fusion device; The preparation method of the transition layer comprises the following steps: S11: adding the epoxidized hydroxyapatite and sulfolane prepared in Comparative Example 2 into a reaction kettle and dispersing them evenly, controlling the temperature to 210° C., and obtaining a solution A; S12: adding the phosphorylated PEEK and sulfolane prepared in Comparative Example 2 into a reaction kettle and heating to 250° C., stirring and dissolving, adding solution A under heat preservation conditions and dispersing evenly to obtain a transition layer slurry; S13: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature at 270°C, sintering for 15 minutes, controlling the temperature at 170°C, and heat treating for 12 hours to obtain a transition layer with a thickness of 125 μm, wherein the epoxidized hydroxyapatite accounts for 30 wt%; The preparation method of hydroxyapatite coating comprises the following steps: S21: mixing the nano-hydroxyapatite prepared in Comparative Example 1 with distilled water to obtain a suspension, wherein the solid content of the suspension is 15%; S22: The suspension was sprayed using plasma spraying technology (gas flow rate 180 L / min, arc current 180 A, spraying distance 80 mm) to obtain a hydroxyapatite coating with a thickness of 75 um.
[0038] Comparative Example 4 Compared with Example 6, Comparative Example 4 is characterized in that only the epoxidized hydroxyapatite prepared in Example 3 used in preparing the transition layer in Example 6 is replaced by an equal amount of hydroxyapatite prepared in Example 1. The remaining components and preparation method in Comparative Example 4 are exactly the same as those in Example 6.
[0039] Comparative Example 5 Compared with Example 6, Comparative Example 5 only replaces an equal amount of the phosphorylated PEEK prepared in Example 3 used in preparing the transition layer in Example 6 with PEEK resin (PEEK 450PF powder produced by Victrex Company of the United Kingdom), and the remaining components and preparation method in Comparative Example 5 are exactly the same as those in Example 6.
[0040] Comparative Example 6 See also Figure 1The atlantoaxial PEEK intervertebral fusion device comprises a device body 1, a developing pin 2 for intraoperative developing and positioning, and a composite coating 3; the device body is made of PEEK resin (PEEK 450PF powder produced by Victrex, UK), and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; the composite coating is a hydroxyapatite coating; The composite coating is a composite coating on the tooth surface of the atlantoaxial PEEK interbody fusion device, including a hydroxyapatite coating coated on the pre-treated tooth surface of the atlantoaxial PEEK interbody fusion device; The preparation method for pre-treating the tooth surface of the atlantoaxial PEEK intervertebral fusion device comprises the following steps: The fusion device body 1 was immersed in 85wt% concentrated sulfuric acid at a solid-liquid ratio of 1g:10mL, the temperature was controlled at 60°C, the mixture was stirred and kept warm for 6 hours, ice water was added for washing, and the mixture was dried to obtain a pretreated atlantoaxial PEEK interbody fusion device; The preparation method of hydroxyapatite coating comprises the following steps: S21: mixing the nano-hydroxyapatite prepared in Example 1 and distilled water to obtain a suspension, wherein the solid content of the suspension is 15%; S22: The suspension was sprayed using plasma spraying technology (gas flow rate 180 L / min, arc current 180 A, spraying distance 80 mm) to obtain a hydroxyapatite coating with a thickness of 200 um.
[0041] Comparative Example 7 See also Figure 1 The atlantoaxial PEEK intervertebral fusion device includes a device body 1, a developing pin 2 for intraoperative imaging positioning, and a composite coating 3; the device body is made of PEEK resin (PEEK 450PF powder produced by Victrex, UK), and the contact surface between the device body and the vertebral body is designed with a tooth-shaped structure for preventing the product from retreating; the composite coating is coated on the surface of the tooth-shaped structure; The composite coating is a composite coating on the tooth surface of the atlantoaxial PEEK interbody fusion device, including a transition layer coated on the tooth surface of the atlantoaxial PEEK interbody fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method of the transition layer comprises the following steps: S11: adding the epoxidized hydroxyapatite and sulfolane prepared in Example 3 into a reaction kettle and dispersing them evenly, controlling the temperature to 210° C., to obtain a solution A; S12: adding the phosphorylated PEEK and sulfolane prepared in Example 3 into a reaction kettle and heating to 250° C., stirring and dissolving, adding solution A under heat preservation conditions and dispersing evenly to obtain a transition layer slurry; S13: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature at 270°C, sintering for 15 minutes, controlling the temperature at 170°C, and heat treating for 12 hours to obtain a transition layer with a thickness of 125 μm, wherein the epoxidized hydroxyapatite accounts for 30 wt%; The preparation method of hydroxyapatite coating comprises the following steps: S21: mixing the nano-hydroxyapatite prepared in Example 1 and distilled water to obtain a suspension, wherein the solid content of the suspension is 15%; S22: The suspension was sprayed using plasma spraying technology (gas flow rate 180 L / min, arc current 180 A, spraying distance 80 mm) to obtain a hydroxyapatite coating with a thickness of 75 um.
[0042] Performance Testing (1) Contact angle: The SL2008 water contact instrument was used to test the contact angle. A 2uL deionized water droplet was freely dropped from a needle (OD=1mm, ID=0.82mm) onto the surface of the composite coating. The angle between the solid and liquid interfaces when the droplet was stabilized on the auxiliary material surface was measured as the water contact angle. The test results are shown in Table 1. (2) Bonding strength: The bonding strength of the coating was tested using a WS-2005 coating adhesion automatic scratch tester. The critical load was evaluated based on the acoustic emission signal captured in the scratch test. The indenter slid on the coating surface and the load was continuously increased during the process. When the critical value Lc (critical load) was reached, the coating and the substrate began to peel off. At this time, the critical load was the coating bonding strength. The test results are shown in Table 1. (3) Solubility: Record the weight of the sample when it is dry (W) 干 The sample was immersed in a centrifuge tube filled with 50 mL phosphate buffer (PBS) for 21 days and then taken out to dry. The mass loss of the coating was calculated. The test results are shown in Table 1: Prepare phosphate buffer: 1000mL PBS contains 8.0g NaCl, 0.2g KCl, 1.4g Na2HPO4, 0.2g KH2PO4 dissolved in 1000mL distilled water, adjust the pH to 4 with 1mol / L citric acid, sterilize by high pressure, and store at 4℃; Table 1: Statistical table of mechanical properties test data of Examples 5-7 and Comparative Examples 3-7
[0043] As can be seen from Table 1, the hydroxyapatite prepared in this application is used as the raw material of the hydroxyapatite coating. The hydrophilic properties of the coating are effectively adjusted by doping with fluoride ions. The contact angle of the coating prepared in Examples 5-7 of this application is close to 70°, which is the most suitable angle for cell adhesion and can accelerate cell migration; this application effectively adjusts the problem of hydroxyapatite and PEEK due to the difference in mechanical properties, which causes the coating to fall off easily, by setting a transition layer between the hydroxyapatite coating and the PEEK substrate. The prepared material can be used in biological organisms for a long time. In addition, the water absorption rate and swelling rate of the material prepared in this application in PBS for 16 days are both 0%, and there is no change in mass and volume, that is, in the body fluid environment, the material structure and function of the material prepared in this application are stable, ensuring support and reconstruction of the surrounding bone tissue.
[0044] (4) Biocompatibility Cell culture: MC3T3-E1 cells (mouse embryonic osteoblast precursor cells purchased from Wuhan Pronocell) were selected and cultured in a serum cell culture medium (DMEM) containing 89% DMEM+F12, 10% fetal bovine serum (FBS), 1% penicillin and streptomycin in a sterile incubator at 37°C, 5% CO2 concentration, and 95% humidity; ①Cell proliferation detection The materials prepared in Examples 5-7 and Comparative Examples 3-7 were placed in a 24-well plate and MC3T3-E1 cells were cultured at 5×10 3 / mL / well density was seeded on the material, and the liquid volume in each well was 1mL. The well plate was gently washed with PBS on days 1, 3, and 7, and then the cell proliferation was measured with the CCK-8 kit. The details are as follows: CCK-8 storage solution was prepared as a working solution (premixed) with ordinary culture medium at a ratio of 1:10, and then the working solution was added to the sample well plate at 100uL per well. At the same time, a blank well plate was set up and 100uL was added to each well for control, and then incubated in a 37°C incubator for 2.5h. Finally, the incubated liquid was transferred to a 96-well plate and placed on an ELx800 microplate reader to measure its absorbance at 450nm. The absorbance value of the sample well plate minus the absorbance value of the blank well plate reflects its proliferation; the test results are shown in Table 3; ② Cytotoxicity assay The materials prepared in Examples 5-7 and Comparative Examples 3-7 were placed in a 24-well plate and MC3T3-E1 cells were cultured at a rate of 1×10 4 / ml / well density on the material, each well has a liquid volume of 1mL, and the plate is gently washed with PBS after 24h, and then the cytotoxicity is detected with the Calcein-AM / PI cell double staining kit. The details are as follows: According to the instructions, Calcein-AM and PI are added to PBS to prepare a working solution, so that the final concentration is 2μM and 4.5μM, and the amount of liquid added to each well is based on the thin slice. Stain at room temperature for 15min, avoid light throughout the process, and finally observe with a fluorescence microscope; Cytotoxicity is reflected by relative growth rate (RGR), and the cytotoxicity standard of RGR determination is shown in Table 2, and the test results are shown in Table 3; Table 2: Cytotoxicity criteria for RGR assay
[0045] Table 3: Statistical table of biocompatibility test data of Examples 5-7 and Comparative Examples 3-7
[0046] It can be seen from Table 3 that MC3T3-E1 cells are cultured on the surfaces of the coatings prepared in Examples 5-7 and Comparative Examples 3-7 of the present application. It can be seen that the coatings prepared in the present application provide an environment that is conducive to the attachment of osteoblasts and have optimal cell proliferation activity, which can promote the initial adhesion and spreading of osteoblasts on the surface of the material, and is conducive to the further growth of osteoblasts and the rapid formation of initial bone tissue.
[0047] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A composite coating on the tooth surface of an atlantoaxial PEEK intervertebral fusion device, characterized in that: It includes a transition layer coated on the tooth surface of the atlantoaxial PEEK interbody fusion device and a hydroxyapatite coating on the surface of the transition layer; The preparation method of the transition layer comprises the following steps: S1: Add epoxidized hydroxyapatite and sulfolane into a reaction kettle and disperse them evenly, and control the temperature at 210-220° C. to obtain solution A; S2: Phosphorylated PEEK and sulfolane are added into a reactor, heated and stirred to dissolve, and solution A is added under heat preservation conditions to disperse evenly to obtain a transition layer slurry; S3: coating the transition layer slurry on the tooth surface of the atlantoaxial PEEK interbody fusion device, sintering at high temperature, and heat treating to obtain the transition layer; The preparation method of epoxidized hydroxyapatite comprises the following steps: Add anhydrous ethanol and deionized water into a reaction kettle and disperse them evenly, adjust the pH to 4-5, add γ-glycidyloxypropyltriethoxysilane, stir at room temperature for 0.5-1h, add nano-hydroxyapatite, control the temperature at 60-65°C, keep warm and stir for 2-4h, filter, wash with water, and dry to obtain epoxidized hydroxyapatite; The preparation method of the phosphorylated PEEK comprises the following steps: A1: Add polyetheretherketone and concentrated sulfuric acid into a reaction kettle, control the temperature at 0-5°C, disperse until the solution becomes transparent, add chloromethyloctyl ether, keep warm and stir for 1-3 hours, add ice water to stop the reaction, filter, wash with water until neutral, wash with ethanol, and dry to obtain component 1; A2: Add component 1 and N-methylpyrrolidone into the reaction kettle and disperse them evenly, add triethyl phosphite, control the temperature at 110-120°C, keep the reaction warm for 12-18 hours, remove triethyl phosphite by vacuum distillation, wash with water, dry, add concentrated hydrochloric acid, heat and reflux for 9-15 hours, filter, wash with water, and dry to obtain phosphorylated PEEK.
2. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 1, characterized in that: The epoxidized hydroxyapatite accounts for 30-50% of the total mass of the transition layer.
3. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 1, characterized in that: The thickness of the transition layer is 15-125 um.
4. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 1, characterized in that: The addition ratio of anhydrous ethanol, deionized water, γ-glycidyloxypropyltriethoxysilane and nano-hydroxyapatite is 45-90mL: 5-10mL: 2.5-5mL: 1g.
5. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 1, characterized in that: The addition ratio of polyetheretherketone, concentrated sulfuric acid and chloromethyloctyl ether in A1 is 1g:50-75mL:8-15mL.
6. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 1, characterized in that: The addition ratio of component 1, N-methylpyrrolidone and triethyl phosphite in A2 is 1g:20-40mL:2-4mL.
7. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 1, characterized in that: The hydroxyapatite coating is made of nano-hydroxyapatite as a raw material and is prepared into a suspension, which is obtained by plasma spraying technology. The thickness of the hydroxyapatite coating is 45-75um.
8. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to any one of claims 1 or 7, characterized in that: The preparation method of hydroxyapatite comprises the following steps: 0.5-2.5 mol / L calcium nitrate tetrahydrate aqueous solution, 0.5-3 mol / L diammonium hydrogen phosphate aqueous solution and ammonium fluoride are mixed, the pH value is adjusted to 9-10, the temperature is controlled at 60-90° C., the reaction is carried out by heat preservation, filtration, aging for 24-48 hours, and deionized water dialyzing to remove ammonia and salt to obtain nano hydroxyapatite.
9. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to claim 8, characterized in that: Calcium nitrate tetrahydrate aqueous solution, diammonium hydrogen phosphate aqueous solution, and ammonium fluoride were prepared according to the molar ratio of Ca:P:F of 16.7:10:
1.
10. The atlantoaxial PEEK intervertebral fusion device tooth surface composite coating according to any one of claims 1 to 7, characterized in that: The transition layer is applied on the surface of the PEEK component of the atlantoaxial PEEK intervertebral fusion device; the PEEK component is obtained by subjecting PEEK resin to surface sulfonation treatment.
Citation Information
Patent Citations
Personalized 3D printing interbody fusion cage and preparation method thereof
CN108606860A
Articular cartilage repair
CN109789020A
Preparation method of biodegradable interbody fusion cage surface bioactive coating and product thereof
CN110624131A
3D printing manufacturing method of artificial skull restoration
CN110639059A
Hydroxyapatite coating based on polyether-ether-ketone and preparation method thereof
CN113633824A