Seawater recycling high-power concentration membrane preparation method and membrane element
Through the preparation method of seawater resource-based high-power concentrated film, the temperature ladder controls and controls the interface polymerization reaction speed, the problems of limited increase in the concentration ratio of salt solution in the seawater desalination industry are solved, and efficient high-power concentrated and simple process design are achieved. .
Patent Information
- Application Number
- CN202410990064.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the high-efficiency concentration ratio combined with the chemical salt industry is limited, and the concentration point of the salt solution is difficult to increase, and the operating pressure is high and the process design is complex, making it difficult to achieve high-efficiency concentration.
A high-power concentrated film preparation method is adopted to prepare a high-power concentrated film by cast film liquid preparation, base film preparation, water-phase preparation and oil-phase preparation, combined with temperature step control, the interface polymerization reaction speed is regulated, and a high-power concentrated film is prepared to realize the salt solution. efficient concentration.
High-power concentration of the salt solution is achieved, with a concentration point of up to 300,000 ppm, reducing operating pressure and process complexity, simplifying process design, and suitable for engineering applications.
Smart Images

Figure CN118904087A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concentration membranes, and in particular to a method for preparing a high-concentration membrane for seawater resource utilization and a membrane element. Background Art
[0002] At present, combining the desalination industry with the chemical salt production industry to achieve efficient concentration is the key to realizing the comprehensive utilization of concentrated seawater. The existing pressure-driven reverse osmosis membrane components have limited concentration multiples for concentrated seawater. The concentration point of the spiral reverse osmosis membrane element for the salt solution is 100,000 ppm, and the flat reverse osmosis can reach 120,000 ppm. The fundamental reason is that it is difficult to overcome the osmotic pressure of the salt solution.
[0003] In the related technology, relevant research has been conducted on membrane materials and processes. Some research works reduce the osmotic pressure by sacrificing seawater desalination membrane desalination (it is difficult to effectively overcome the osmotic pressure due to the limited reduction of membrane material desalination), and some research works achieve high-fold concentration through combined processes. The preliminary work has made certain progress, and the concentration point of the salt solution can reach 150,000 ppm. Composite membrane is a very important type of nanofiltration separation membrane. Due to its stable structure and operating performance, it has become the most commercialized type of nanofiltration membrane. Among them, the structure of the composite membrane is divided into a porous support layer in the lower layer and an ultra-thin selective cortex in the upper layer. It is generally believed that the support layer in the lower layer provides mechanical strength for the composite membrane, while the selective cortex in the upper layer determines the separation performance of the composite membrane. At present, most composite nanofiltration membranes are prepared by interfacial polymerization. However, the existing technology has technical problems such as limited improvement of the concentration multiple of the salt solution, excessively high operating pressure (high energy consumption) and complex process design that is difficult to apply in engineering. How to overcome the osmotic pressure of high-concentration salt solutions and simplify process design are key issues in achieving high-fold concentration. Summary of the invention
[0004] To this end, the present invention provides a method for preparing a high-concentration membrane for seawater resource utilization and a membrane element, which solves the problems of limited concentration multiples of salt solutions, excessively high operating pressure (high energy consumption) and complex process design that are difficult to apply in engineering in traditional technologies.
[0005] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a high-concentration membrane for seawater resource utilization, comprising the following steps:
[0006] Preparation of the casting solution: polysulfone of a specified concentration, an additive of a specified concentration and a first solvent of a specified concentration are placed in a mixing kettle, the materials in the mixing kettle are heated to a first set temperature, the materials in the mixing kettle are stirred at a first preset stirring speed for a first specified time; then stirred at a second preset stirring speed for a second specified time; stirred at a third preset stirring speed for a third specified time under negative pressure; when the material temperature in the mixing kettle reaches the second set temperature, the materials are allowed to stand for degassing for a fourth specified time to obtain the casting solution;
[0007] Preparation of base film: coating the prepared casting solution on the non-woven fabric, and preparing the base film combining the non-woven fabric and polysulfone through phase inversion;
[0008] Preparation of aqueous phase: adding a specified concentration of amine monomer, a specified concentration of polypiperazine and a specified concentration of acid binding agent to pure water, stirring and dissolving at 20-40° C. for a fifth specified time to obtain a mixed solution, and standing for a sixth specified time to obtain an aqueous phase solution for standby use;
[0009] Preparation of the oil phase: adding the oil phase monomer of the specified concentration to the second solvent, stirring at room temperature for the seventh specified time, and standing for the eighth specified time to obtain an oil phase solution for use;
[0010] Preparation of composite membrane: Coat the surface of the base membrane with an aqueous solution, use a pressure roller and an air knife to remove excess water on the surface of the base membrane, then slit-extrusion-coat the oil solution to a specified thickness, remove excess oil by passing through an oil pressure roller, and then pass through a temperature step control platform area to regulate the rate of the interfacial polymerization reaction to obtain a highly concentrated membrane.
[0011] As a preferred method for preparing a high-concentration membrane for seawater resource utilization, during the preparation of the casting solution:
[0012] The additive is selected from at least one of pure water, small molecule ketones, small molecule alcohols, polyvinyl alcohol with a specified molecular weight, and polyvinyl pyrrolidone with a specified molecular weight;
[0013] The first solvent is selected from at least one of dimethylformamide, dimethylacetamide and dimethyl sulfoxide.
[0014] As a preferred method for preparing a high-concentration membrane for seawater resource utilization, during the preparation of the base membrane:
[0015] Non-woven fabrics should be made of polyolefin or polytetrafluoroethylene acid and alkali resistant materials.
[0016] As a preferred solution for the method of preparing a high-concentration membrane for seawater resource utilization, the thickness of the non-woven fabric is 30-100 microns, and the pore size of the non-woven fabric is 0.01-0.5 microns.
[0017] As a preferred solution for the preparation of high-concentration membrane for seawater resource utilization, during the water phase preparation process:
[0018] The ratio of amine monomer to polypiperazine is controlled between 50:1 and 1:1, and the back-end step oven process is used to adjust the thickness of the functional layer and the desalination rate.
[0019] As a preferred solution for the preparation of a high-concentration membrane for seawater resource utilization, an acid-binding agent is used to absorb the acid generated in the interface process to promote the forward reaction.
[0020] As a preferred solution for the preparation of a high-concentration membrane for seawater resource utilization, the amine monomer is selected from polyethyleneimine, polyethyleneamine, polypiperidine, m-phenylenediamine, p-phenylenediamine or similar derivatives.
[0021] As a preferred solution for the preparation method of high-concentration membrane for seawater resource utilization, triethylamine, pyridine and the like are selected as acid-binding agents.
[0022] As a preferred solution for the preparation of high-concentration membrane for seawater resource utilization, during the preparation of the oil phase:
[0023] The second solvent is one or more of ParG, IsoparG, IsoparE, IsoparM, pentane and alkanes with more than one carbon atom;
[0024] The oil phase monomer is trimesoyl chloride and its derivatives.
[0025] The present invention also provides a seawater resource recovery high-concentration membrane element, comprising a high-concentration membrane prepared by the above-mentioned seawater resource recovery high-concentration membrane preparation method, wherein the pure water flow channel thereof is divided into regions with double wavy rubber lines.
[0026] The beneficial effects of the present invention are as follows: the present invention implements temperature step control to regulate the speed of interfacial polymerization reaction, the initial reaction is relatively mild and the subsequent reaction is violent, the desalination of the functional layer is controllable and thicker, and the product can be guaranteed to be resistant to high pressure; the concentration membrane of the present invention can balance the water inlet / water production pressure difference, and high-fold concentration can be achieved simply and efficiently. The concentration point of the salt solution can reach 300,000 ppm. There is no need to reduce the osmotic pressure by sacrificing seawater desalination membrane desalination or to achieve high-fold concentration by a combined process. The process design is simpler, which is conducive to engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0028] Figure 1 A schematic diagram of a process for preparing a high-concentration membrane for seawater resource utilization provided in an embodiment of the present invention;
[0029] Figure 2 Electron microscope photos of the surface and cross section of a high-power concentration membrane obtained by the method for preparing a high-power concentration membrane for seawater resource utilization provided in an embodiment of the present invention;
[0030] Figure 3 It is a schematic diagram of the design of the high-concentration membrane element for seawater resource utilization provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0031] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] See also Figure 1 The embodiment of the present invention provides a method for preparing a high-concentration membrane for seawater resource utilization, comprising the following steps:
[0033] S1, preparing a casting solution: putting polysulfone of a specified concentration, an additive of a specified concentration, and a first solvent of a specified concentration into a mixing kettle, heating the materials in the mixing kettle to a first set temperature, stirring the materials in the mixing kettle at a first preset stirring speed for a first specified time; then stirring at a second preset stirring speed for a second specified time; stirring at a third preset stirring speed for a third specified time under negative pressure; when the material temperature in the mixing kettle reaches the second set temperature, standing and degassing for a fourth specified time to obtain a casting solution;
[0034] S2, base film preparation: coating the prepared casting solution on the non-woven fabric, and preparing a base film combining the non-woven fabric and polysulfone through phase inversion;
[0035] S3, water phase preparation: add a specified concentration of amine monomer, a specified concentration of polypiperazine and a specified concentration of acid binding agent to pure water, stir and dissolve at 20-40° C. for a fifth specified time to obtain a mixed solution, let stand for a sixth specified time to obtain an aqueous phase solution for standby;
[0036] S4, oil phase preparation: adding a specified concentration of oil phase monomer to the second solvent, stirring at room temperature for a seventh specified time, and standing for an eighth specified time to obtain an oil phase solution for standby use;
[0037] S5. Preparation of composite membrane: Coat the surface of the base membrane with an aqueous solution, use a pressure roller and an air knife to remove excess water on the surface of the base membrane, then slit-extrusion-coat the oil solution to a specified thickness, remove excess oil by passing through an oil pressure roller, and then pass through a temperature step control platform area to regulate the rate of interfacial polymerization reaction to obtain a highly concentrated membrane.
[0038] Specifically, in step S1, 20wt% polysulfone, 1wt% polyvinylpyrrolidone (PVP) and 79wt% dimethylformamide (DMF) are put into a mixing kettle, and the oil furnace (the oil furnace is used to provide a heat source for heating the mixing kettle) is heated to a set oil furnace temperature of 95°C; the stirring speed is 60Hz; the stirring time is 8h; then, 50Hz rapid stirring is performed within the first 10min; then 10Hz slow negative pressure stirring is used for stirring for 6h; when the material temperature reaches 25°C, it is allowed to stand for degassing for 12h.
[0039] The additives in the casting solution can be pure water, small molecule ketones, small molecule alcohols, polyvinyl alcohols of different molecular weights, polyvinyl pyrrolidones of different molecular weights, etc., with a content of 0-3%. The balance is a solvent, which is at least one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, etc.
[0040] Specifically, in step S2, the prepared casting solution is applied to a PET-based non-woven fabric, and then a base film of a combination of a non-woven fabric and polysulfone is prepared by phase inversion. The non-woven fabric can be made of polyethylene terephthalate, polyethylene, polypropylene and other polyolefins or polytetrafluoroethylene and other acid and alkali resistant materials, with a thickness of 30-100 microns and a pore size of 0.01-0.5 microns.
[0041] Specifically, in step S3, 1-5wt% m-phenylenediamine, 0.1-1wt% polypiperazine and 0.5-2.0wt% triethylamine are added to pure water and stirred at 20-40°C for 2h to dissolve to obtain a mixed solution, which is then allowed to stand for 1h for standby use. The ratio of m-phenylenediamine to polypiperazine is controlled between 50:1 and 1:1 and the back-end step oven process is used to adjust the thickness of the functional layer and the desalination rate; triethylamine absorbs the acid generated in the interface process and promotes the forward reaction.
[0042] In addition, the amine monomers may be polyethyleneimine, polyethyleneamine, polypiperidine, m-phenylenediamine, p-phenylenediamine or other similar derivatives; the acid-binding agent may be triethylamine, pyridine and the like.
[0043] Specifically, in step S4, poly(trimethylol) chloride is added to the ParG solvent, accounting for 0.5wt% of the total mass, and stirred at room temperature for 1 hour, and then allowed to stand for 1 hour for standby use. Wherein, ParG is a mixed solvent of alkanes, and the solvent can be selected from IsoparG, IsoparE, IsoparM, and can also be selected from one or more (isomers) of pentane and alkanes with carbon atoms above (≤C16); the oil phase monomer can be trimesoyl chloride and its derivatives, with a content of 0.5-5wt.%.
[0044] Specifically, in step S5, the surface of the base film is coated with an aqueous solution, and after 1 minute, the excess aqueous phase on the surface is removed using a pressure roller and an air knife, and then the oil phase solution is slit extrusion coated with a thickness of 200um, and the excess oil phase is removed by an oil phase pressure roller. On its surface, a temperature step control platform area is passed, and the platform area can achieve a 20℃-100℃ gradient of 10℃ precise control, regulate the interface polymerization reaction speed, and achieve a more uniform and thicker functional layer, which can ensure product uniformity and pressure resistance. The cross-section and surface structure of the composite membrane are as follows Figure 2 As shown, the thickness of the composite layer is effectively increased compared to the traditional nanofiltration membrane, reaching 100-200nm to achieve high pressure resistance.
[0045] See also Figure 3 Another embodiment of the present invention further provides a high-concentration membrane element for seawater resource utilization, including a high-concentration membrane prepared by a method for preparing a high-concentration membrane for seawater resource utilization according to the above embodiment, wherein the pure water flow channel thereof is divided into regions with double wavy rubber lines.
[0046] The conventional reverse osmosis membrane element process is: slitting of the flow channel cloth, processing of the central tube, slitting of the membrane, pre-assembly, film rolling, and curing and cutting of the finished product. There are two main differences between the roll-type forward osmosis membrane element and the reverse osmosis membrane element: one is that the central tube is dead, one section is water inlet and the other section is water production; the other is that the pure water flow channel is glued on three sides, and a longitudinal glue is applied along the dead position of the central tube. In this embodiment, based on the forward osmosis membrane element, the above-mentioned high-concentration membrane is adopted. On the one hand, the glue line is designed to be wavy, and the dilute salt solution enters the pure water diversion network through the opening of the central tube. By increasing the flow rate, the dilute salt solution and the composite membrane water production are evenly mixed. The mixed solution enters the right area with a reduced flow rate, which is conducive to further mixing, and then flows out through the right central tube. On the other hand, double wavy glue lines are applied in different areas to further improve the mixing of the dilute salt solution and the produced water, offset the transmembrane osmotic pressure, and help the subsequent high-concentration.
[0047] Based on the above-mentioned method for preparing a high-concentration membrane for seawater resource utilization and a membrane element in the embodiment of the present invention, the following test case was designed to demonstrate the technical effect of the present invention.
[0048] Test case 1
[0049] Prepare m-phenylenediamine and piperazine in a certain proportion (total amount 5.0wt.%), add 1.0wt% triethylamine, stir at 20-40°C for 2h to fully dissolve to obtain a water phase mixture, and then let it stand for 1h for standby use. Add 0.5wt% trimesoyl chloride to ParG solvent, stir at 20-40°C for 2h to obtain an oil phase mixture, and then let it stand for 1 hour for standby use. Use a pre-cast base film (thickness of 140±3 microns), after being immersed in the pre-prepared water phase, enter the water phase pressure roller / air knife, enter the platform area, and then enter the slit extrusion oil phase quantitative coating process for spraying, control the coating speed of 10m / min, the coating amount of 200ml / min and the oven treatment temperature of 80°C to obtain a composite film for standby use.
[0050] Table 1 Effect of mixed monomer ratio on basic properties of composite membrane
[0051]
[0052] In Table 1, MPD is m-phenylenediamine and PIP is piperazine. Test conditions: 800psi, 32000ppm. As can be seen from Table 1, as the MPD:PIP ratio increases, the sodium chloride desalination increases from 55.4% to 98.5%, and the flux decreases from 140LMH to 25LMH. The two mixed monomers participate in the interfacial polymerization process. When the MPD:PIP ratio is high, the MPD containing primary amines dominates and forms a dense functional layer; as the MPD:PIP ratio decreases, the two monomers have a competition mechanism, and the functional layer gradually becomes loose.
[0053] Test case 2
[0054] In the test case 1, based on the MPD:PIP ratio of 3:1, the temperature in the oven was adjusted in steps to obtain a composite membrane for use.
[0055] Table 2 Effect of step temperature difference on basic performance and structure of composite membrane
[0056] Control method NaCl flux LMH NaCl desalination rate % Functional layer thickness nm B-Blank 65 78.5 100 B-1 56 75..6 150 B-2 45 72.4 200 B-3 30 71.8 300
[0057] In Table 2, B-0 represents a normal oven at 80°C, B-1 represents a step increase from 20°C to 80°C at 30°C, B-2 represents a step increase from 20°C to 80°C at 20°C, and B-3 represents a step increase from 20°C to 80°C at 10°C. Test conditions: 1Mpa, 2000ppmMgSO4. As can be seen from Table 2, the oven section adopts temperature step control, and the desalination of the composite membrane is slightly reduced compared with the blank sample (the desalination is reduced from 78.5% to 71.8%), the flux is significantly reduced (from 65LMH to 30LMH), and the thickness of the functional layer is significantly increased. The temperature step control process can effectively control the reaction process. The initial low temperature can effectively overcome the volatilization of the water phase on the surface of the base membrane and provide sufficient water phase monomers for interfacial polymerization; at the same time, it can avoid the uneven volatilization of the water phase on the surface of the base membrane, which will affect the uniformity of the composite membrane.
[0058] Test case 3
[0059] Conditions B-0 and B-2 in Test Case 2 were selected to test the operating stability of the membrane material under high pressure. The specific results are shown in Table 3. The test conditions in Table 3 are: 5.6 MPa, 32000 ppm NaCl. The high pressure resistance test was carried out using two membrane materials, B-0 and B-2.
[0060] Table 3 Comparison of pressure resistance of different composite membranes
[0061]
[0062] As can be seen from Table 3, after running for 90 days at 5.6 MPa and 32000 ppm NaCl, the flux and desalination of the B-2 membrane material changed very little, while the flux and desalination of the B-0 membrane material changed greatly. The good operating stability of B-2 under high pressure is mainly determined by its high thickness functional layer.
[0063] Test case 4
[0064] The concentration multiples and operating pressures of two membrane elements were tested under high salt and high pressure. One element was a rolled seawater desalination reverse osmosis membrane, and the other was a high-concentration membrane element rolled using B-2 diaphragm and the above-mentioned pure water flow channel.
[0065] Table 4 Concentration of brine by two membrane elements
[0066]
[0067] In Table 4, the test conditions use 32000ppm NaCl; wherein, the salt solution of the central tube inlet of the high-concentration reverse osmosis membrane element is adjustable. It can be concluded from Table 4 that the use of a rolled seawater membrane element can concentrate 32000ppm concentrated brine to 100,000, and the operating pressure reaches 10MPa. The high-concentration membrane element prepared by the technology of the present invention can achieve high concentration under low osmotic pressure by regulating the salt concentration and recovery rate at the inlet of the central tube, and can be concentrated to 200,000ppm.
[0068] In summary, the present invention puts polysulfone of a specified concentration, an additive of a specified concentration, and a first solvent of a specified concentration into a mixing kettle, heats the materials in the mixing kettle to a first set temperature, stirs the materials in the mixing kettle at a first preset stirring speed for a first specified time; then stirs at a second preset stirring speed for a second specified time; stirs at a third preset stirring speed for a third specified time under negative pressure; when the material temperature in the mixing kettle reaches the second set temperature, stands for degassing for a fourth specified time to obtain a casting solution; applies the prepared casting solution on a non-woven fabric, and prepares a base film combining the non-woven fabric and polysulfone through phase inversion; adds a specified concentration of pure water to the mixture; Amine monomers of a specified concentration, polypiperazine of a specified concentration and an acid binding agent of a specified concentration are stirred and dissolved at 20-40° C. for a fifth specified time to obtain a mixed solution, which is allowed to stand for a sixth specified time to obtain an aqueous phase solution for standby use; an oil phase monomer of a specified concentration is added to the second solvent, stirred at room temperature for a seventh specified time, and allowed to stand for an eighth specified time to obtain an oil phase solution for standby use; the aqueous phase solution is coated on the surface of the base film, excess water phase on the surface of the base film is removed by a pressure roller and an air knife, and then the oil phase solution is slit extrusion-coated to a specified thickness, excess oil phase is removed by an oil phase pressure roller, and then the temperature is passed through a step control platform area to regulate the interface polymerization reaction rate to obtain a high-concentration membrane. The present invention implements temperature step control to regulate the speed of interfacial polymerization reaction. The initial reaction is relatively mild while the subsequent reaction is intense, so that the desalination of the functional layer is controllable and thicker, and the product can be guaranteed to be resistant to high pressure. The concentration membrane of the present invention can balance the water inlet / water production pressure difference, and achieve high-fold concentration simply and efficiently. The concentration point of the salt solution can reach 300,000 ppm. There is no need to reduce the osmotic pressure by sacrificing seawater desalination membrane desalination or to achieve high-fold concentration by a combined process. The process design is simpler, which is conducive to engineering applications.
[0069] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.
Claims
1. A method for preparing a high-concentration membrane for seawater resource utilization, It is characterized in that The following steps are involved: Preparation of the casting solution: polysulfone of a specified concentration, an additive of a specified concentration and a first solvent of a specified concentration are placed in a mixing kettle, the materials in the mixing kettle are heated to a first set temperature, the materials in the mixing kettle are stirred at a first preset stirring speed for a first specified time; then stirred at a second preset stirring speed for a second specified time; stirred at a third preset stirring speed for a third specified time under negative pressure; when the material temperature in the mixing kettle reaches the second set temperature, the materials are allowed to stand for degassing for a fourth specified time to obtain the casting solution; Preparation of base film: coating the prepared casting solution on the non-woven fabric, and preparing the base film combining the non-woven fabric and polysulfone through phase inversion; Preparation of aqueous phase: adding a specified concentration of amine monomer, a specified concentration of polypiperazine and a specified concentration of acid binding agent to pure water, stirring and dissolving at 20-40° C. for a fifth specified time to obtain a mixed solution, and standing for a sixth specified time to obtain an aqueous phase solution for standby use; Preparation of the oil phase: adding the oil phase monomer of the specified concentration to the second solvent, stirring at room temperature for the seventh specified time, and standing for the eighth specified time to obtain an oil phase solution for use; Preparation of composite membrane: Coat the surface of the base membrane with an aqueous solution, use a pressure roller and an air knife to remove excess water on the surface of the base membrane, then slit-extrusion-coat the oil solution to a specified thickness, remove excess oil by passing through an oil pressure roller, and then pass through a temperature step control platform area to regulate the rate of the interfacial polymerization reaction to obtain a highly concentrated membrane.
2. The method for preparing a high-concentration membrane for seawater resource utilization according to claim 1, It is characterized in that During the preparation of the casting solution: The additive is selected from at least one of pure water, small molecule ketones, small molecule alcohols, polyvinyl alcohol with a specified molecular weight, and polyvinyl pyrrolidone with a specified molecular weight; The first solvent is selected from at least one of dimethylformamide, dimethylacetamide and dimethyl sulfoxide.
3. The method for preparing a high-concentration membrane for seawater resource utilization according to claim 1, It is characterized in that During the preparation of the basement membrane: Non-woven fabrics should be made of polyolefin or polytetrafluoroethylene acid and alkali resistant materials.
4. A method for preparing a high-concentration membrane for seawater resource utilization according to claim 3, It is characterized in that The thickness of the non-woven fabric is 30-100 microns, and the pore size of the non-woven fabric is 0.01-0.5 microns.
5. The method for preparing a high-concentration membrane for seawater resource utilization according to claim 1, It is characterized in that During the water phase preparation process: The ratio of amine monomer to polypiperazine is controlled between 50:1 and 1:1, and the back-end step oven process is used to adjust the thickness of the functional layer and the desalination rate.
6. A method for preparing a high-concentration membrane for seawater resource utilization according to claim 5, It is characterized in that Acid binding agents are used to absorb the acid generated during the interfacial process and promote the forward reaction.
7. The method for preparing a high-concentration membrane for seawater resource utilization according to claim 6, It is characterized in that The amine monomers are polyethyleneimine, polyethyleneamine, polypiperidine, m-phenylenediamine, p-phenylenediamine or similar derivatives.
8. The method for preparing a high-concentration membrane for seawater resource utilization according to claim 7, It is characterized in that The acid binding agent is selected from triethylamine, pyridine and the like.
9. The method for preparing a high-concentration membrane for seawater resource utilization according to claim 1, It is characterized in that During the oil phase preparation process: The second solvent is one or more of ParG, IsoparG, IsoparE, IsoparM, pentane and alkanes with more than one carbon atom; The oil phase monomer is trimesoyl chloride and its derivatives.
10. A high-concentration membrane element for seawater resource utilization, comprising a high-concentration membrane prepared by the method for preparing a high-concentration membrane for seawater resource utilization according to any one of claims 1 to 9, It is characterized in that The pure water flow channel is divided into areas with double wavy rubber lines.
Citation Information
Patent Citations
Preparation method of polyvinyl alcohol ultrathin selective layer nanofiltration membrane
CN113828165A
Nanofiltration membrane and preparation method thereof
CN115646212A
Pollution-resistant conductive nanofiltration membrane as well as preparation method and application thereof