Preparation method of high-flux zirconium oxide-titanium oxide composite ceramic nanofiltration membrane

Zr-Ti composite sol is prepared by sol-microwave hydrothermal method, combined with microwave hydrothermal and drying and calcining steps, the agglomeration and shrinkage problems caused by irregular morphology of powder materials in ceramic membranes are solved, and high-throughput oxidation is achieved The high-quality preparation of zirconium-titanium oxide ceramic nanofiltration membrane improves the separation efficiency and mechanical strength of the membrane.

CN118904108APending Publication Date: 2024-11-08SUNTAR MEMBRANE TECHNOLOGY (XIAMEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964187.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing ceramic film preparation methods, irregular morphology of powder materials leads to uneven mass transfer stress, agglomeration phenomenon and anisotropic shrinkage affect the separation efficiency and mechanical strength of the film, making it difficult to obtain a film with uniform pore size distribution.

Method used

The Zr-Ti composite sol was prepared by sol-microwave hydrothermal method, and a high-throughput zirconia-titanium oxide ceramic nanofiltration membrane was directly formed on the ceramic membrane support through microwave hydrothermal reaction and drying and calcining steps, and a high-throughput zirconia-titanium oxide ceramic nanofiltration membrane was directly formed on the ceramic membrane support, using glycerol additives Optimize the growth process of nanoparticles to ensure uniformity and integrity of the membrane layer.

Benefits of technology

The performance of the ceramic membrane is significantly improved, a uniform porosity and mechanical strength is formed, the preparation steps are simplified, the production cycle is shortened, and complex coating and sintering processes are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904108A_ABST
    Figure CN118904108A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-flux zirconium oxide-titanium oxide composite ceramic nanofiltration membrane, which adopts a modified sol-microwave hydrothermal method to generate a titanium oxide film on an aluminum oxide substrate in situ, and forms a composite nanofiltration membrane layer through a low-temperature calcination process. The nanofiltration membrane with excellent separation performance is successfully prepared through efficient, low-cost and simplified steps, and the method is suitable for various industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiltration membrane preparation, and specifically relates to a method for preparing a high-flux zirconium oxide-titanium oxide composite ceramic nanofiltration membrane. Background Art

[0002] Ceramic membranes have won wide attention in the field of separation technology and are widely used in many industrial processes due to their excellent chemical stability, high mechanical strength, high temperature resistance, resistance to microbial corrosion and long service life. These advantages make ceramic membranes an ideal choice for treating various fluids, including corrosive or high-temperature media.

[0003] There are various methods for preparing ceramic membranes, including chemical vapor deposition, anodization, sol-gel, and solid particle sintering. Each method has its specific application scenarios and technical advantages. However, in actual production, commonly used powder materials often have irregular morphology problems. This irregularity will lead to uneven mass transfer forces during particle sintering, which will cause agglomeration between particles. Agglomeration will not only generate cracks, but may also form an uneven pore structure, which will lead to the generation of some dead holes or semi-through holes, thereby affecting the separation efficiency and selectivity of the membrane.

[0004] During the sintering process, the anisotropic shrinkage of the powder particles will also have an adverse effect on the pore structure. This shrinkage may not only lead to stress concentration inside the membrane layer, but also cause cracks, thereby reducing the integrity and mechanical strength of the membrane. In addition, anisotropic shrinkage will also affect the precise control of the pore structure, making it more difficult to obtain a membrane with a uniform pore size distribution. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a high-flux zirconium oxide-titania composite ceramic nanofiltration membrane.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing a high-flux zirconium oxide-titania composite ceramic nanofiltration membrane comprises the following steps:

[0008] (1) adding glycerol to a solution containing an organic zirconium alkoxide and an organic titanium alkoxide, performing a hydrolysis reaction at 60-80° C. with stirring for 2-3 hours, then performing solid-liquid separation, re-dispersing the solid in water, adding nitric acid for peptization and adjusting the pH value of the peptized solution to 1-2, and preparing a Zr-Ti composite sol; in the above solution, the molar ratio of Zr to Ti is 0.1-0.5:1;

[0009] (2) placing the Zr-Ti composite sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 50-80%, and then immersing the pretreated ceramic membrane support in the Zr-Ti composite sol in the microwave hydrothermal reaction device, and reacting at a pressure of 0.5-2 MPa for 1-3 hours, and cooling to obtain a wet zirconium oxide-titania ceramic nanofiltration membrane;

[0010] (3) The wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 80-120° C. at a humidity of 10-20%, kept warm and dried for 2-5 hours, then heated to 350-500° C., kept warm and calcined for 2-5 hours, and cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

[0011] In a preferred embodiment of the present invention, the organic zirconium alkoxide is zirconium isopropoxide or zirconium n-butoxide.

[0012] More preferably, the organic zirconium alkoxide is zirconium isopropoxide.

[0013] In a preferred embodiment of the present invention, the organic titanium alkoxide is titanium isopropoxide or titanium n-butoxide.

[0014] More preferably, the organic titanium alkoxide is titanium n-butoxide.

[0015] In a preferred embodiment of the present invention, the organic zirconium alkoxide is zirconium isopropoxide or zirconium n-butoxide, and the organic titanium alkoxide is titanium isopropoxide or titanium n-butoxide.

[0016] More preferably, the organic zirconium alkoxide is zirconium isopropoxide, and the organic titanium alkoxide is titanium n-butoxide.

[0017] In a preferred embodiment of the present invention, in the solution of step (1), the concentration of the organic zirconium alkoxide is 0.01-0.05 mol / L, and the concentration of the organic titanium alkoxide is 0.1 mol / L.

[0018] Further preferably, in the solution of step (1), the final concentration of glycerol is 0.05 mol / L.

[0019] In a preferred embodiment of the present invention, the step (3) is as follows: the wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 80-120°C at a rate of 1-3°C / min at a humidity of 10-20%, and then kept warm and dried for 2-5 hours, and then heated to 350-500°C at a rate of 1-5°C / min, kept warm and calcined for 2-5 hours, and cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

[0020] The beneficial effects of the present invention are:

[0021] 1. The present invention adopts the sol-microwave hydrothermal method to successfully prepare the Zr-Ti composite sol, and based on it, develops a high-quality zirconium oxide-titanium oxide ceramic nanofiltration membrane. The present invention cleverly combines the fine nanoparticle preparation technology of the sol with the rapid and uniform heating characteristics of the microwave hydrothermal method, significantly improving the performance of the ceramic nanofiltration membrane.

[0022] 2. The Zr-Ti composite sol prepared by the sol-microwave hydrothermal method of the present invention exhibits the remarkable advantages of fine grains, uniform particle size, complete crystal development and no agglomeration. These characteristics are crucial for forming a ceramic membrane with a uniform pore structure. The present invention not only improves the stability of titanium dioxide nanoparticles by doping zirconium ions, but also restrains the growth of TiO2 grains to a certain extent, slows down the overall densification process of the porous ceramic membrane, and thus effectively improves the porosity of the porous ceramic membrane.

[0023] 3. In order to solve the problem that particles tend to grow larger during microwave hydrothermal process, the present invention specially adds glycerol additive and adopts mixed doping method. This not only optimizes the growth process of nanoparticles, but also ensures the uniformity and integrity of the composite film layer. By directly loading the zirconium oxide-titania composite film layer on the base film, and after drying and calcining steps, we successfully prepared defect-free, high-quality zirconium oxide-titania ceramic nanofiltration membrane.

[0024] 4. The process flow of the present invention has significant advantages, including simplified preparation steps, shortened production cycle and improved production efficiency. Compared with the traditional sol-gel method, the present invention avoids the complicated coating and sintering process, realizes the in-situ preparation of Zr-Ti film, and directly obtains the zirconium oxide-titania nanofiltration membrane layer. In addition, through the combination of modified sol-gel method and microwave hydrothermal reaction, the present invention can directly load the zirconium oxide-titania film on the substrate in a relatively short time, and prepare a high-quality nanofiltration membrane through the drying and calcining steps. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope photograph of the high-flux zirconium oxide-titania ceramic nanofiltration membrane prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0027] Example 1

[0028] (1) adding glycerol with a final concentration of 0.05 mol / L to a solution containing zirconium isopropoxide with a concentration of 0.01 mol / L and titanium n-butoxide with a concentration of 0.1 mol / L, performing a hydrolysis reaction at room temperature under stirring for 2 h, then performing suction filtration to achieve solid-liquid separation, re-dissolving the obtained filter cake layer in water, adding acid for peptization and making the pH value of the peptized solution 1, to obtain a Zr-Ti composite sol;

[0029] (2) placing the Zr-Ti composite sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the pretreated ceramic membrane support in the Zr-Ti composite sol in the microwave hydrothermal reaction device, and reacting at a pressure of 0.5 MPa for 2 hours, and cooling to obtain a wet zirconium oxide-titania ceramic nanofiltration membrane;

[0030] (3) The wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

[0031] The high flux zirconia-titania ceramic nanofiltration membrane prepared in this example is as follows Figure 1 As shown, the membrane layer is intact. Under the test conditions of room temperature and 0.69 MPa, the rejection rate for 2 g / L PEG (molecular weight 600) is 95%, and the flux is 70 LHM.

[0032] Example 2

[0033] (1) adding glycerol with a final concentration of 0.05 mol / L to a solution containing zirconium isopropoxide with a concentration of 0.02 mol / L and titanium n-butoxide with a concentration of 0.1 mol / L, performing a hydrolysis reaction at room temperature for 2 h, then performing suction filtration to achieve solid-liquid separation, re-dissolving the obtained filter cake layer in water, adding acid for peptization and making the pH value of the peptized solution 1, to obtain a Zr-Ti composite sol;

[0034] (2) placing the Zr-Ti composite sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the pretreated ceramic membrane support in the Zr-Ti composite sol in the microwave hydrothermal reaction device, and reacting at a pressure of 0.5 MPa for 2 hours, and cooling to obtain a wet zirconium oxide-titania ceramic nanofiltration membrane;

[0035] (3) The wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

[0036] The high-flux zirconium oxide-titania ceramic nanofiltration membrane prepared in this example has a retention rate of 97% for 2 g / L PEG (molecular weight 600) and a flux of 75 LHM under the test conditions of room temperature and 0.69 MPa.

[0037] Example 3

[0038] (1) adding glycerol with a final concentration of 0.05 mol / L to a solution containing zirconium isopropoxide with a concentration of 0.05 mol / L and titanium n-butoxide with a concentration of 0.1 mol / L, performing a hydrolysis reaction at room temperature for 2 h, then performing suction filtration to achieve solid-liquid separation, re-dissolving the obtained filter cake layer in water, adding acid for peptization and making the pH value of the peptized solution 1, to obtain a Zr-Ti composite sol;

[0039] (2) placing the Zr-Ti composite sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the pretreated ceramic membrane support in the Zr-Ti composite sol in the microwave hydrothermal reaction device, and reacting at a pressure of 0.5 MPa for 2 hours, and cooling to obtain a wet zirconium oxide-titania ceramic nanofiltration membrane;

[0040] (3) The wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

[0041] The high-flux zirconium oxide-titania ceramic nanofiltration membrane prepared in this example has a retention rate of 92% for 2 g / L PEG (molecular weight 1000) and a flux of 80 LHM under the test conditions of room temperature and 0.69 MPa.

[0042] Example 4

[0043] (1) adding glycerol with a final concentration of 0.05 mol / L to a solution containing zirconium isopropoxide with a concentration of 0.01 mol / L and titanium n-butoxide with a concentration of 0.1 mol / L, performing a hydrolysis reaction at room temperature under stirring for 2 h, then performing suction filtration to achieve solid-liquid separation, re-dissolving the obtained filter cake layer in water, adding acid for peptization and making the pH value of the peptized solution 1, to obtain a Zr-Ti composite sol;

[0044] (2) placing the Zr-Ti composite sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the pretreated ceramic membrane support in the Zr-Ti composite sol in the microwave hydrothermal reaction device, and reacting at a pressure of 2 MPa for 2 h, and cooling to obtain a wet zirconium oxide-titania ceramic nanofiltration membrane;

[0045] (3) The wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

[0046] The high-flux zirconium oxide-titania ceramic nanofiltration membrane prepared in this example has a retention rate of 90% for 2 g / L PEG (molecular weight 600) and a flux of 82 LHM under the test conditions of room temperature and 0.69 MPa.

[0047] Comparative Example 1

[0048] (1) adding glycerol with a final concentration of 0.05 mol / L to a solution containing titanium n-butoxide with a concentration of 0.1 mol / L, performing a hydrolysis reaction at room temperature under stirring for 2 h, then performing suction filtration to achieve solid-liquid separation, re-dissolving the obtained filter cake layer in water, adding acid for peptization and making the pH value of the peptized solution 1, to obtain a Ti sol;

[0049] (2) placing the Ti sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the pretreated ceramic membrane in the Ti sol in the microwave hydrothermal reaction device, and reacting at a pressure of 0.5 MPa for 2 hours, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0050] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a comparative ceramic nanofiltration membrane.

[0051] The comparative ceramic nanofiltration membrane prepared in this comparative example has a retention rate of 90% for 2 g / L PEG (molecular weight 600) and a flux of 46 LHM under the test conditions of room temperature and 0.69 MPa.

[0052] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing a high-flux zirconium oxide-titania composite ceramic nanofiltration membrane, characterized in that: The steps include: (1) adding glycerol to a solution containing an organic zirconium alkoxide and an organic titanium alkoxide, performing a hydrolysis reaction at 60-80° C. with stirring for 2-3 hours, then performing solid-liquid separation, re-dispersing the solid in water, adding nitric acid for peptization and adjusting the pH value of the peptized solution to 1-2, and preparing a Zr-Ti composite sol; in the above solution, the molar ratio of Zr to Ti is 0.1-0.5:1; (2) placing the Zr-Ti composite sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 50-80%, and then immersing the pretreated ceramic membrane support in the Zr-Ti composite sol in the microwave hydrothermal reaction device, and reacting at a pressure of 0.5-2 MPa for 1-3 hours, and cooling to obtain a wet zirconium oxide-titania ceramic nanofiltration membrane; (3) The wet zirconia-titania ceramic nanofiltration membrane prepared in step (2) is heated to 80-120° C. at a humidity of 10-20%, kept warm and dried for 2-5 hours, then heated to 350-500° C., kept warm and calcined for 2-5 hours, and cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.

2. The preparation method according to claim 1, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide or zirconium n-butoxide.

3. The preparation method according to claim 2, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide.

4. The preparation method according to claim 1, characterized in that: The organic titanium alkoxide is titanium isopropoxide or titanium n-butoxide.

5. The preparation method according to claim 4, characterized in that: The organic titanium alkoxide is titanium n-butoxide.

6. The preparation method according to claim 1, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide or zirconium n-butoxide, and the organic titanium alkoxide is titanium isopropoxide or titanium n-butoxide.

7. The preparation method according to claim 6, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide, and the organic titanium alkoxide is titanium n-butoxide.

8. The preparation method according to any one of claims 1 to 7, characterized in that: In the solution of step (1), the concentration of the organic zirconium alkoxide is 0.01-0.05 mol / L, and the concentration of the organic titanium alkoxide is 0.1 mol / L.

9. The preparation method according to claim 8, characterized in that: In the solution of step (1), the final concentration of glycerol is 0.05 mol / L.

10. The preparation method according to any one of claims 1 to 7, characterized in that: The step (3) is as follows: the wet zirconia-titania ceramic nanofiltration membrane obtained in step (2) is heated to 80-120°C at a rate of 1-3°C / min at a humidity of 10-20%, and is kept warm and dried for 2-5 hours, and then heated to 350-500°C at a rate of 1-5°C / min, and is kept warm and calcined for 2-5 hours, and cooled to obtain a high-flux zirconia-titania ceramic nanofiltration membrane.