Preparation method and application of activated manganese dioxide and sulfenyl functional group synergistic functionalized biochar composite material

By loading active manganese dioxide and sulfur-based functional groups on biochar, forming a synergistic functional composite material, the adsorption effect and stability problems caused by the modification of single metal functional groups and sulfur-containing functional groups are solved, and high efficiency for a variety of heavy metals is achieved Removal and material stability improve.

CN118904282APending Publication Date: 2024-11-08NORTHWEST A & F UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410768031.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, when dealing with heavy metal contaminants, a single metal functional group cannot meet the efficient removal of multiple metal cations, and the modification of sulfur-containing functional group causes biochar stability problems, and the adsorption effect is limited.

Method used

Directed doping technology is used to support active manganese dioxide and sulfur-based functional groups on biochar to form a synergistic functionalized biochar composite material for active manganese dioxide and sulfur-based functional groups, improving adsorption performance and enhancing stability.

Benefits of technology

It significantly improves the removal ability of mercury and lead pollutants, solves the problem of unstable aggregation of activated manganese oxide fine particles and the binding of sulfur-based functional groups, realizes the efficient removal effect of multifunctional biochar composites, and reduces the risk of loss. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904282A_ABST
    Figure CN118904282A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of an active manganese dioxide and sulfenyl functional group synergistic functional charcoal composite material. The biochar composite material is prepared by directionally introducing active manganese dioxide particles and sulfur-containing functional groups to a biochar crude product obtained by pyrolyzing agricultural and forestry organic wastes, and the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material with a layered porous structure is prepared. The active manganese dioxide and sulfenyl functional group synergistic functional charcoal composite material can be used for repairing mercury and lead pollution in a water body or soil, the content of mercury and lead in the water body and the toxicity of mercury and lead in the soil can be remarkably reduced, and extraction of mercury and lead by vegetable crops is reduced while the soil fertility is increased; the method has the characteristics of good economic benefit, simple preparation method, reusability, large-area popularization and application and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental pollution remediation, and specifically relates to a preparation method and application of a composite material of active manganese dioxide and sulfur-based functional groups synergistically functionalized biochar. Background Art

[0002] Heavy metal pollutants, especially mercury and lead, are typical pollutants in wastewater produced by non-ferrous metal smelting, because the high toxicity of mercury and the high content of lead have attracted widespread attention. These heavy metals can enter the soil, surface and groundwater, and mercury and lead in water and soil environments mainly exist in the form of divalent ions or minerals through leaching, sedimentation and runoff, which can easily cause serious water and soil pollution, damage the ecological environment, and thus cause harm to human health.

[0003] At present, the engineering methods for treating these pollutants are roughly divided into bioremediation technology, chemical remediation technology and physical remediation technology. The adsorption method in physical remediation technology is the most effective, economical and mature method for treating low-concentration pollutants. Adsorption materials include chemical polymers, natural minerals, metal-based substances and carbon-based products. Chemical polymers have brought challenges to practical engineering applications due to their relatively high cost; natural minerals are the earliest materials used for metal pollution in water and soil. They are widely used due to their low price and high surface area, but the release of associated minerals and impurities poses a high risk of secondary pollution; metal-based substances have large surface energy and are easy to form aggregates in water and soil, thus affecting the adsorption effect of mercury and lead; and the adsorption effect of pure carbon-based adsorbents is limited by the number of surface functional groups, and the range of pollutants treated is very narrow. Therefore, considering the adsorption effect, economic feasibility and environmental friendliness, it is necessary to develop new green adsorbents.

[0004] Pyrolysis of biomass in an oxygen-free environment helps to convert most organic compounds into highly aromatic, carbon-rich, and insoluble solid porous biochar with excellent stability. Biochar shows excellent prospects as an adsorbent, but the adsorption capacity of unmodified biochar for heavy metals essentially depends on factors such as the physicochemical properties of the biomass and the specific pyrolysis temperature of the precursor. Generally, biochar obtained by pyrolysis at temperatures above 600°C shows good hydrophilicity, which provides a prerequisite for the removal of mercury and lead in water and soil, but due to the lack of functional groups in the matrix and surface, it has limited attraction to mercury and lead.

[0005] Manganese dioxide is a low-cost, high-specific surface area, environmentally friendly material with affinity for multiple metals. With better heavy metal adsorption capacity than iron oxides and outstanding catalytic effect on redox reactions, it performs well in various environmental applications. However, there are few reports on loading specific forms of manganese dioxide (including α, β, γ, δ and λ) on the surface of carbon materials. Among them, α-manganese dioxide is the crystal form with the strongest adsorption capacity and catalytic activity. Since the introduction of a single metal functional group may not meet the requirements of efficient removal of multiple metal cations at the same time, multifunctional modification is a sustainable approach. The strong Lewis acid-base interaction between sulfur-containing groups and heavy metal ions has made it an excellent choice for improving the adsorption performance of carbon-based materials. Therefore, introducing sulfur-containing groups to the surface of biochar for the removal of mercury in water and soil is a promising idea. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a preparation method and application of a composite material of biochar with synergistic functionalization of active manganese dioxide and sulfur-based functional groups in view of the deficiencies of the above-mentioned prior art. The present invention uses agricultural and forestry organic waste to prepare biochar with high porosity and high surface hydrophilicity, and loads active manganese dioxide and sulfur-containing groups onto biochar through directional doping technology to prepare a composite material of biochar with multifunctional active manganese dioxide and sulfur-based functional groups; the metal nanoparticles in the composite material improve the interfacial chemical properties of the carbon-based material while also providing more binding sites for the sulfur-containing functions, solving the problem that the introduction of a single metal functional group cannot meet the requirements of efficient removal of multiple metal cations at the same time, and the problem of biochar stability caused by the modification of a single sulfur-containing functional group.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0008] A method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups comprises the following steps:

[0009] S1. Mix the agricultural and forestry organic waste with the pore-forming agent, grind it thoroughly, seal it and place it for 12 to 24 hours, dry it, and then heat it to 600 to 650°C at a rate of 5 to 10°C / min in an inert atmosphere, pyrolyze it for 1.5 to 2 hours, and cool it to obtain a crude biochar product assisted by molten salt pyrolysis;

[0010] S2, adding the crude biochar obtained by molten salt-assisted pyrolysis in S1 to a manganese salt solution, stirring evenly, to obtain a suspension 1; adding the suspension 1 to an alkaline solution containing manganese oxalate, stirring evenly, to obtain a suspension 2; then transferring the suspension 2 to an autoclave, oxidizing and crystallizing at a pressure of 3 MPa and a temperature of 200° C. for 20 to 24 hours, cooling and standing, washing and drying the obtained solid matter, and obtaining an active manganese dioxide enhanced molten salt-assisted pyrolysis biochar material;

[0011] S3. The active manganese dioxide enhanced molten salt assisted pyrolysis biochar material obtained in S2 is mixed with sulfur and ground to form a mixture powder; the mixture powder is then heated to 400-450°C at a rate of 5-10°C / min under an inert atmosphere, pyrolyzed for 15-20min, cooled, washed and dried to obtain a biochar composite material synergistically functionalized with active manganese dioxide and sulfur-based functional groups.

[0012] Preferably, the agricultural and forestry organic waste in S1 includes ground powder of straw, wood chips, leaves, branches, etc.; the pore-forming agent is one of sodium hydroxide, potassium hydroxide or sodium carbonate; and the mass ratio of the agricultural and forestry organic waste to the pore-forming agent is 3:1.

[0013] Preferably, the manganese salt solution in S2 is manganese chloride tetrahydrate or manganese sulfate tetrahydrate solution, with a concentration of 0.1 mol / L; the ratio of the crude biochar from the molten salt-assisted pyrolysis to the manganese salt solution is 1 g:5 mL;

[0014] Preferably, the alkaline solution containing manganese oxalate in S2 is a sodium hydroxide solution with a concentration of 0.5 mol / L, and the molar number of manganese oxalate dissolved therein is the same as that of the manganese salt solution; the ratio of the crude biochar produced by molten salt assisted pyrolysis to the alkaline solution containing manganese oxalate is 1 g:25 mL.

[0015] Preferably, the stirring speed in S2 is 180 r / min; the solid material is washed with deionized water for 3 to 4 times and then dried at 105° C. for 6 to 8 hours.

[0016] Preferably, the sulfur element described in S3 is one of sublimated sulfur or sulfur; and the mass ratio of the activated manganese dioxide enhanced molten salt assisted pyrolysis biochar material to the sulfur element is 1:1.

[0017] Preferably, after the mixture powder in S3 is pyrolyzed and cooled, it is washed with deionized water for 4 to 5 times and then dried at 105° C. for 6 to 8 hours.

[0018] The present invention also provides an active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material prepared by the above preparation method.

[0019] The present invention also provides the use of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material in removing mercury and / or lead pollutants.

[0020] Preferably, the regeneration method of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material comprises the following steps:

[0021] The active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material adsorbing mercury and / or lead pollutants are mixed with a desorption solution and stirred for 4 to 6 hours; the desorption solution is a hydrochloric acid solution with a concentration of 1 mol / L.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention loads active manganese dioxide and sulfur-based functional groups on biochar materials by directional doping technology to prepare manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite materials, which can solve the problems of aggregation of active manganese dioxide fine particles in liquid phase systems and low adsorption efficiency, and at the same time solve the problem of unstable combination of non-metallic functional groups and biochar. While improving the dispersibility of active manganese dioxide fine particles, it adds unreported synergistic functionalization of sulfur-based functional groups, so that it has better mercury and lead pollutant removal capabilities, and can also effectively reduce the loss of active manganese dioxide fine particles and sulfur-based functional groups.

[0024] 2. Agricultural and forestry organic waste (such as straw, wood chips, leaves, branches, etc.) is produced in large quantities on a daily basis, has a high organic matter content, and improper treatment can easily cause environmental pollution. The present invention uses such agricultural and forestry organic waste as raw materials, which can be obtained in large quantities without investing additional costs. The agricultural and forestry organic waste is pyrolyzed to prepare biochar materials, which can convert waste into resources with application value, and has good adsorption capacity for high-risk heavy metal pollutants, and has potential engineering application value.

[0025] 3. The raw materials and reagents used in the present invention are low-cost, green and pollution-free, and the preparation method of the biochar composite material synergistically functionalized by active manganese dioxide and sulfur-based functional groups is simple to operate, has low equipment requirements, and is suitable for large-scale promotion.

[0026] 4. The active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material of the present invention can be used to remove mercury and lead pollutants in water or soil, and has the advantages of low cost, good effect, strong operability, no secondary pollution, beautification of the environment, etc. In addition, due to the loading of metal oxides, the active manganese dioxide and sulfur-based functional group multifunctional biochar composite material after adsorbing mercury and lead pollutants is easy to separate from the polluted medium, and can be regenerated and recycled.

[0027] 5. The activated manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material prepared by the present invention has the characteristics of being green and pollution-free: in the process of material regeneration, the used hydrochloric acid desorption solution can be used to form a solid precipitate containing mercury and lead by adding alkali; if the activated manganese dioxide and sulfur-based functional group multifunctional biochar composite material cannot meet the demand for removing mercury and lead pollutants after repeated use, it can be directly incinerated to obtain a solid residue containing manganese, mercury and lead. These solid precipitates or solid residues containing manganese, mercury and lead can be used as mineral raw materials for the recovery of elements such as manganese, mercury and lead or sent to a hazardous waste treatment center for treatment.

[0028] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is an X-ray crystal diffraction (XRD) spectrum of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material of Example 1 of the present invention;

[0030] Figure 2 is a scanning electron microscope (SEM) image of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material of Example 1 of the present invention;

[0031] Figure 3 This is an energy dispersive X-ray spectrometer (EDS) elemental composition distribution spectrum of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material of Example 1 of the present invention;

[0032] Figure 4 These are the adsorption data and model fitting of mercury and lead at different initial concentrations by the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material of Example 5 of the present invention.

[0033] Figure 5 This is a recycling efficiency diagram of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material of Example 5 of the present invention.

[0034] Figure 6 This is the effect of adding active manganese dioxide and sulfur-based functional groups to synergistically functionalize the biochar composite material in Example 7 of the present invention on the biomass of planted spinach. DETAILED DESCRIPTION

[0035] Example 1

[0036] This embodiment is a method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups, comprising the following steps:

[0037] S1. Rinse the agricultural and forestry organic waste (10% leaves, 90% sawdust), dry it at 105°C, crush it, add NaOH solid at a mass ratio of 3:1, grind it thoroughly, seal it and let it stand for 12 hours, put it into a porcelain crucible and compact it, transfer it into a temperature-controlled muffle furnace, set the program to increase the temperature to 600°C at a gradient of 5°C / min under inert conditions, pyrolyze it for 1.5 hours, cool it to room temperature and take it out to obtain the crude biochar assisted by molten salt pyrolysis.

[0038] S2. Mix 20 g of the crude biochar obtained by molten salt-assisted pyrolysis in S1 with 100 mL of a 0.1 mol / L MnCl2·4H2O solution, stir evenly, and form a homogeneous suspension 1; add MnC2O4 to a 0.5 mol / L NaOH solution to make the MnC2O4 concentration 0.02 mol / L to obtain an alkaline solution containing manganese oxalate, and then transfer the suspension 1 to 500 mL of an alkaline solution containing manganese oxalate, stir evenly at a speed of 180 r / min to obtain a new suspension 2; then transfer the suspension 2 to an autoclave and oxidize and crystallize at a pressure of 3 MPa and a temperature of 200°C for 24 hours, cool and stand, wash the obtained solid material with deionized water 3 times, and then dry it at 105°C for 6 hours to obtain an active manganese dioxide enhanced molten salt-assisted pyrolysis biochar material.

[0039] S3. Weigh the activated manganese dioxide enhanced molten salt-assisted pyrolysis biochar material and sublimated sulfur obtained in S2 in a mass ratio of 1:1, place them in a ceramic crucible, grind and fully mix them to form a mixture powder; wrap the mixture powder with tin foil and put it into a temperature-controlled muffle furnace. Under inert conditions, set the program to increase the temperature to 450°C at a gradient of 10°C / min, pyrolyze for 15 minutes, and take out after cooling to room temperature; wash with deionized water 4 times, and dry at 105°C for 6 hours to obtain a biochar composite material with synergistic functionalization of active manganese dioxide and sulfur-based functional groups.

[0040] The X-ray diffraction (XRD) analysis of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material obtained in this example shows Figure 1 It was found that α-manganese dioxide (referred to as active manganese dioxide in the present invention) crystals were introduced into the interior of the biochar matrix.

[0041] The active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material obtained in this example was scanned by scanning electron microscopy (SEM). Figure 2 , and energy dispersive X-ray spectrometer (EDS) analysis, such as Figure 3It was found that the active manganese dioxide particles and sulfur-containing functional groups in the biochar composite material doped with active manganese dioxide and sulfur-based functional groups were successfully dispersed on the surface of the composite material, and the prepared active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material was a porous core-shell carbon composite material.

[0042] Example 2

[0043] This embodiment is a method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups, comprising the following steps:

[0044] S1. Rinse the agricultural and forestry organic waste (20% straw, 80% sawdust), dry it at 105°C, crush it, add KOH solid at a mass ratio of 3:1, grind it thoroughly, seal it and let it stand for 12 hours, put it into a porcelain crucible and compact it, transfer it into a temperature-controlled muffle furnace, set the program to increase the temperature to 600°C at a gradient of 5°C / min under inert conditions, pyrolyze it for 1.5 hours, cool it to room temperature and take it out to obtain the crude biochar assisted by molten salt pyrolysis.

[0045] S2. Mix 20 g of the crude biochar obtained by molten salt-assisted pyrolysis in S1 with 100 mL of a 0.1 mol / L MnSO4·4H2O solution, stir evenly, and form a homogeneous suspension 1; add MnC2O4 to a 0.5 mol / L NaOH solution to make the MnC2O4 concentration 0.02 mol / L to obtain an alkaline solution containing manganese oxalate, and then transfer the suspension 1 to 500 mL of an alkaline solution containing manganese oxalate, stir evenly at a speed of 180 r / min to obtain a new suspension 2; then transfer the suspension 2 to an autoclave and oxidize and crystallize at a pressure of 3 MPa and a temperature of 200°C for 24 hours, cool and stand, wash the obtained solid material with deionized water 3 times, and then dry it at 105°C for 8 hours to obtain an active manganese dioxide enhanced molten salt-assisted pyrolysis biochar material.

[0046] S3. Weigh the activated manganese dioxide enhanced molten salt-assisted pyrolysis biochar material and sulfur obtained in S2 in a mass ratio of 1:1, place them in a ceramic crucible, grind and fully mix them to form a mixture powder; wrap the mixture powder with tin foil and put it into a temperature-controlled muffle furnace. Under inert conditions, set the program to increase the temperature to 450°C at a gradient of 10°C / min, pyrolyze for 15 minutes, and take out after cooling to room temperature; wash with deionized water 5 times, and dry at 105°C for 6 hours to obtain a biochar composite material with synergistic functionalization of active manganese dioxide and sulfur-based functional groups.

[0047] Example 3

[0048] This embodiment is a method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups, comprising the following steps:

[0049] S1. Rinse the agricultural and forestry organic waste (25% leaves, 75% branches), dry it at 105℃, crush it, add Na2CO3 solid in a mass ratio of 3:1, grind it thoroughly, seal it and let it stand for 18 hours, put it into a porcelain crucible and compact it, transfer it into a temperature-controlled muffle furnace, set the program to increase the temperature to 650℃ at a gradient of 5℃ / min under inert conditions, pyrolyze it for 1.5 hours, cool it to room temperature and take it out to obtain the crude biochar assisted by molten salt pyrolysis.

[0050] S2. Mix 20 g of the crude biochar obtained by molten salt-assisted pyrolysis in S1 with 100 mL of a 0.1 mol / L MnSO4·4H2O solution, stir evenly, and form a homogeneous suspension 1; add MnC2O4 to a 0.5 mol / L NaOH solution to make the MnC2O4 concentration 0.02 mol / L to obtain an alkaline solution containing manganese oxalate, and then transfer the suspension 1 to 500 mL of an alkaline solution containing manganese oxalate, stir evenly at a speed of 180 r / min to obtain a new suspension 2; then transfer the suspension 2 to an autoclave and oxidize and crystallize at a pressure of 3 MPa and a temperature of 200°C for 20 hours, cool and stand, wash the obtained solid material with deionized water 4 times, and then dry it at 105°C for 8 hours to obtain an active manganese dioxide enhanced molten salt-assisted pyrolysis biochar material.

[0051] S3. Weigh the activated manganese dioxide enhanced molten salt-assisted pyrolysis biochar material and sulfur obtained in S2 in a mass ratio of 1:1, place them in a ceramic crucible, grind and fully mix them to form a mixture powder; wrap the mixture powder with tin foil and put it into a temperature-controlled muffle furnace. Under inert conditions, set the program to increase the temperature to 400°C at a gradient of 5°C / min, pyrolyze for 15 minutes, and take out after cooling to room temperature; wash with deionized water 4 times, and dry at 105°C for 8 hours to obtain a biochar composite material with synergistic functionalization of activated manganese dioxide and sulfur-based functional groups.

[0052] Example 4

[0053] This embodiment is a method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups, comprising the following steps:

[0054] S1. Rinse the agricultural and forestry organic waste (15% straw, 95% branches), dry it at 105℃, crush it, add NaOH solid at a mass ratio of 3:1, grind it thoroughly, seal it and let it stand for 24 hours, put it into a porcelain crucible and compact it, transfer it into a temperature-controlled muffle furnace, set the program to increase the temperature to 650℃ at a gradient of 10℃ / min under inert conditions, pyrolyze it for 2 hours, cool it to room temperature and take it out to obtain the crude biochar assisted by molten salt pyrolysis.

[0055] S2. Mix 20 g of the crude biochar obtained by molten salt-assisted pyrolysis in S1 with 100 mL of a 0.1 mol / L MnCl2·4H2O solution, stir evenly, and form a homogeneous suspension 1; add MnC2O4 to a 0.5 mol / L NaOH solution to make the MnC2O4 concentration 0.02 mol / L to obtain an alkaline solution containing manganese oxalate, and then transfer the suspension 1 to 500 mL of an alkaline solution containing manganese oxalate, stir evenly at a speed of 180 r / min to obtain a new suspension 2; then transfer the suspension 2 to an autoclave and oxidize and crystallize at a pressure of 3 MPa and a temperature of 200°C for 22 hours, cool and stand, wash the obtained solid material with deionized water 3 times, and then dry it at 105°C for 6 hours to obtain an active manganese dioxide enhanced molten salt-assisted pyrolysis biochar material.

[0056] S3. Weigh the activated manganese dioxide enhanced molten salt-assisted pyrolysis biochar material and sulfur obtained in S2 in a mass ratio of 1:1, place them in a ceramic crucible, grind and fully mix them to form a mixture powder; wrap the mixture powder with tin foil and put it into a temperature-controlled muffle furnace. Under inert conditions, set the program to increase the temperature to 450°C at a gradient of 10°C / min, pyrolyze for 20 minutes, cool to room temperature and take out; wash with deionized water 5 times, and dry at 105°C for 8 hours to obtain a biochar composite material with synergistic functionalization of activated manganese dioxide and sulfur-based functional groups.

[0057] Example 5

[0058] The performance of the activated manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite materials prepared in Examples 1 to 4 is basically the same, so the following only takes the activated manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material prepared in Example 1 as an example to illustrate its removal effect on mercury and lead pollutants.

[0059] When removing mercury and lead pollutants from water, the active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material prepared in Example 1 was added to a mercury-contaminated water body with a mercury content of 5 to 500 mg / L at a solid-liquid ratio of 2.5 g / L, or was added to a lead-contaminated water body with a lead content of 20 to 1000 mg / L at a solid-liquid ratio of 2.5 g / L; then, at 25°C, the reaction was carried out for 6 to 12 hours to reach adsorption equilibrium. After the contents of mercury and lead in the solution were determined by the standard for the detection of mercury content in water bodies - atomic fluorescence spectrometry (HJ / 694-2014) and the standard for the detection of lead content in water bodies - flame atomic spectrophotometry (GB / T7475-1987), respectively, the active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material was separated from the water body by natural precipitation.

[0060] The adsorption isotherm is Figure 4The results show that when the initial concentration of mercury is 5-100 mg / L or the initial concentration of lead is 20-200 mg / L, the prepared active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material can achieve more than 90% of mercury / lead pollutants in water to be removed. The saturated adsorption capacity of the material for mercury and lead in water is 175.1 mg / g and 228.4 mg / g, respectively.

[0061] The recyclability of the biochar composite material synergistically functionalized with active manganese dioxide and sulfur-based functional groups was evaluated by adsorption-desorption cycle test. First, 100 mg of the sample was immersed in 40 mL of a solution containing mercury (100 mg / L) and lead (150 mg / L) for 24 h; then, it was placed in a 1 mol / L HCl solution and stirred for 4 to 6 h to regenerate the mercury / lead-saturated biochar composite material; after completion, the eluted sample was naturally allowed to stand and precipitate, and then the sample was rinsed with deionized water before the next cycle. The adsorption-desorption cycle was repeated 6 times. The cycle results are shown in Figure 5 As shown, after 6 cycles, the adsorption efficiency of mercury and lead decreased by 25.6% and 12.7%, respectively. Therefore, the number of reuses of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material is 4 to 5 times.

[0062] Example 6

[0063] The active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material prepared in Example 1 was used to study its application in natural water bodies contaminated by mercury and lead.

[0064] Mercuric chloride or lead chloride aqueous solution was added to the collected water samples of Weihe River in Shaanxi and Qujiang River in Xi'an, respectively, to obtain simulated mercury-containing and lead-containing polluted water bodies, namely simulated wastewater; the mercury and lead contents in the simulated wastewater were 0.5-3 mg / L and 5-10 mg / L, respectively. The active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material prepared in Example 1 was added to each simulated wastewater at a solid-liquid ratio of 2.5 g / L for adsorption for 24 hours, and the mercury and lead contents in the water bodies before and after treatment were detected. The results are shown in Table 1.

[0065] Table 1 Adsorption of mercury and lead in simulated natural water by biochar composites

[0066]

[0067]

[0068] As can be seen from Table 1, the test results of the treated river water show that the mercury content is lower than the mercury content limit of 0.01 mg / L in the Pollutant Emission Standard for Recycled Copper, Aluminum, Lead and Zinc Industries (GB31574-2015), and the lead content is lower than the lead content limit of 0.2 mg / L in the Surface Water Environmental Quality Standard (GB3838-2002).

[0069] Example 7

[0070] The active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material prepared in Example 1 was used to study its application in the remediation of mercury-lead composite contaminated soil and the safe production of agricultural products.

[0071] The experimental soil was collected from the soil of medicinal materials planted in Luochuan County, Yan'an City, Shaanxi Province, which was contaminated by mercury and lead. The mercury content in the soil was 5.85 mg / kg, the lead content was 235 mg / kg, and the pH value was 7.99. The experimental group added 1% and 3% of active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite materials to the soil according to the mass ratio, respectively, and the control group was soil without adding composite materials. Three parallels were set for each treatment, and the area of ​​each experimental area was 1m 2 . The top 30 cm of soil in each area was dug out, and the active manganese dioxide and sulfur-based functional group synergistic functionalized biochar prepared in Example 1 were added in proportion. After mixing, the mixture was backfilled to the original position to start passivation. During the cultivation period, the soil moisture content was maintained at about 50%. Soil samples were collected after 30 days of cultivation (20 g was collected from each area), and spinach was immediately planted in the control group and the experimental group. Specifically, 10 seeds were sown in each area, and the seedlings were pulled out and diluted to 4 plants in each area after 15 days. The soil moisture content was maintained at about 45% during the spinach planting period. After 30 days of sowing, the above-ground parts were harvested and rinsed with distilled water. The soil DTPA-extractable mercury / lead content, the different forms of mercury and lead in the rhizosphere soil, and the changes in mercury and lead content in the planted spinach biomass and the edible part of spinach were analyzed through this soil test.

[0072] The DTPA-extractable mercury / lead content in soil was determined by extracting soil samples with diethylenetriaminepentaacetic acid-triethanolamine-calcium chloride dihydrate (DTPA-TEA-CaCl2·2H2O) solution to determine the DTPA-extractable metal concentration in soil. Specifically, 4 g of soil sample was added to 20 mL of DTPA-TEA-CaCl2·2H2O solution and stirred at 180 rpm for 16 h (25±0.2°C); the suspension was then centrifuged at 4000 rpm for 15 min, filtered, and cold atomic fluorescence and flame atomic spectrophotometry were used to obtain DTPA-extractable mercury and lead. The DTPA-extractable mercury and lead concentrations in the control and experimental groups are shown in Table 2.

[0073] Table 2 Concentrations of DTPA-extractable mercury and lead in soil under different treatments

[0074]

[0075] According to Table 2, in the 30-day soil test, it can be found that the Hg and lead contents extracted by DTPA of the biochar composite material synergistically functionalized with 1% and 3% active manganese dioxide and sulfur-based functional groups decreased compared with the initial soil, and the Hg and Pb concentrations decreased by 53.6% to 56.7% and 28.1% to 34.08%, respectively.

[0076] The soils of the control group and the experimental group were extracted by the improved BCR continuous extraction method to observe the forms of Hg and Pb in the soil. 0.5 g of soil sample was accurately weighed in a 50 mL centrifuge tube, and 20 mL of extractants A (0.11 mol / L HNO3), B (0.5 mol / L NH2OH·HCl) and C (8.8 mol / L H2O2 + 1 mol / L NH4OAc) were used for continuous extraction, and the concentrations of mercury and lead in weak acid extraction state, reducible state and oxidizable state were determined respectively. The remaining solid was washed with deionized water, transferred to a digestion tube, and wet digested with nitric acid and perchloric acid at 100 ° C. After completion, the remaining sample was diluted to 20 mL and filtered to determine the concentration of residual mercury and lead. The metal forms in the control soil and the soil added with different proportions of active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composites are shown in Table 3.

[0077] Table 3 Forms of mercury and lead under each treatment

[0078]

[0079]

[0080] As shown in Table 3, the addition of active manganese dioxide and sulfur-based functional groups to synergistically functionalize the biochar composite material promotes the transformation of other forms of metals into a residual state, with the residual state of mercury and lead reaching 26% and 40%, respectively.

[0081] The effect of active manganese dioxide and sulfur-based functional groups on crop growth was evaluated by growing spinach dry biomass. After the spinach was harvested, it was sterilized at 105°C for 30 minutes and then dried at 80°C until constant weight. Three spinach samples with the largest biomass were selected for each treatment, and the average value was taken to represent the biomass under that treatment. Figure 6 As shown in the figure, the dry biomass of spinach harvested under the treatments of adding 1% and 3% composite materials increased by 13.6% and 31.2% respectively compared with the control group. This indicates that the addition of active manganese dioxide and sulfur-based functional groups to synergistically functionalize biochar composites is beneficial to plant growth.

[0082] After the spinach was harvested under each treatment, its edible part was sterilized at 105℃ for 30min, then dried at 80℃ to constant weight, ground and 4g sample was taken, digested by nitric acid-perchloric acid wet digestion method at 100℃ and fixed to 50mL, filtered and 10mL solution was taken for mercury and lead content determination. The heavy metal content of the edible part of the spinach harvested after adding active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composites is shown in Table 4.

[0083] Table 4 Comparison of heavy metal content in edible parts of spinach

[0084]

[0085] As shown in Table 4, the mercury and lead contents in the edible part of spinach planted in the control group soil exceeded the provisions of the National Food Safety Standard for Contaminant Limits in Food (GB2762-2022) for leafy vegetables, which are ≤0.01 mg / kg for mercury and ≤0.3 mg / kg for lead. The edible part of spinach harvested after treatment with 3% active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material meets the above food safety standards.

[0086] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups, characterized in that: The following steps are involved: S1. Mix the agricultural and forestry organic waste with the pore-forming agent, grind it thoroughly, seal it and place it for 12 to 24 hours, then heat it to 600 to 650°C at a rate of 5 to 10°C / min under an inert atmosphere, pyrolyze it for 1.5 to 2 hours, and cool it to obtain a crude biochar product assisted by molten salt pyrolysis; S2, adding the crude biochar obtained by molten salt-assisted pyrolysis in S1 to a manganese salt solution, stirring evenly, to obtain a suspension 1; adding the suspension 1 to an alkaline solution containing manganese oxalate, stirring evenly, to obtain a suspension 2; then transferring the suspension 2 to an autoclave, oxidizing and crystallizing at a pressure of 3 MPa and a temperature of 200° C. for 20 to 24 hours, cooling and standing, washing and drying the obtained solid matter, and obtaining an active manganese dioxide enhanced molten salt-assisted pyrolysis biochar material; S3. The active manganese dioxide enhanced molten salt assisted pyrolysis biochar material obtained in S2 is mixed with sulfur and ground to form a mixture powder; the mixture powder is then heated to 400-450°C at a rate of 5-10°C / min under an inert atmosphere, pyrolyzed for 15-20min, cooled, washed and dried to obtain a biochar composite material synergistically functionalized with active manganese dioxide and sulfur-based functional groups.

2. The method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups according to claim 1, characterized in that: S1 The agricultural and forestry organic waste includes powder obtained by grinding straw, wood chips, leaves and branches; the pore-forming agent is one of sodium hydroxide, potassium hydroxide or sodium carbonate; the mass ratio of the agricultural and forestry organic waste to the pore-forming agent is 3:

1.

3. The method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups according to claim 1, characterized in that: S2: the manganese salt solution is manganese chloride tetrahydrate or manganese sulfate tetrahydrate solution, with a concentration of 0.1 mol / L; the ratio of the crude biochar from the molten salt-assisted pyrolysis to the manganese salt solution is 1 g:5 mL; S2 The alkaline solution containing manganese oxalate is a sodium hydroxide solution with a concentration of 0.5 mol / L, and the molar number of manganese oxalate dissolved therein is the same as that of the manganese salt solution; the ratio of the crude biochar obtained by molten salt assisted pyrolysis to the alkaline solution containing manganese oxalate is 1 g:25 mL.

4. The method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups according to claim 1, characterized in that: S2: The stirring speed is 180 r / min; the solid material is washed with deionized water for 3 to 4 times, and then dried at 105° C. for 6 to 8 hours.

5. The method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups according to claim 1, characterized in that: S3 The sulfur element is sublimated sulfur or one of sulfur; the mass ratio of the activated manganese dioxide enhanced molten salt assisted pyrolysis biochar material to the sulfur element is 1:

1.

6. The method for preparing a composite material of biochar synergistically functionalized by active manganese dioxide and sulfur-based functional groups according to claim 1, characterized in that: S3: After the mixture powder is pyrolyzed and cooled, it is washed with deionized water for 4 to 5 times and then dried at 105° C. for 6 to 8 hours.

7. A composite material of active manganese dioxide and sulfur-based functional groups synergistically functionalized biochar prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the composite material of activated manganese dioxide and sulfur-based functional groups synergistically functionalized biochar according to claim 7 in removing mercury and / or lead pollutants.

9. The use according to claim 8, characterized in that: The regeneration method of the active manganese dioxide and sulfur-based functional group synergistically functionalized biochar composite material comprises the following steps: The active manganese dioxide and sulfur-based functional group synergistic functionalized biochar composite material adsorbing mercury and / or lead pollutants are mixed with a desorption solution and stirred for 4 to 6 hours; the desorption solution is a hydrochloric acid solution with a concentration of 1 mol / L.

Citation Information

Patent Citations

  • Magnetic biochar quantum dot composite adsorbent as well as preparation method and using method thereof

    CN103920461A

  • Manganese dioxide modified biochar composite material as well as a preparation method and an application thereof

    CN107983300A

  • Method for preparing needle-shaped Fe-Mn-S ternary nano-material supported porous charcoal compound material

    CN109225134A

  • Manganese sulfide-phosphoric acid modified biochar composite material as well as preparation method and application thereof

    CN112934177A

  • Soil mercury passivator as well as preparation method and application thereof

    CN114574209A