Method for activating and regenerating decolorized sand
By combining a binder with a method of potassium hydroxide and dilute hydrochloric acid regenerator, the reuse rate and decolorization performance of decolorization sand were successfully improved, and the problem of poor decolorization sand performance in the prior art was solved, and resource conservation and environment were achieved Protect.
Patent Information
- Application Number
- CN202410969858.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Among the existing activation and regeneration methods of decolorized sand, the decolorization performance is poor, the reuse rate is low, the utilization rate is not high, and there are problems of resource waste and environmental pollution.
Using a potassium hydroxide regenerator with a concentration value of 4% to 5% and a dilute hydrochloric acid regenerator with a concentration value of 3% to 6%, combined with an appropriate amount of binder, the waste decolorized sand is regenerated into efficient decolorization through stirring, heating and filtration. Sand, consists of four steps: mixing, stirring, heating and drying, and handling using filters and drying equipment.
It improves the reuse and utilization rate of waste decolorized sand, reduces resource waste and environmental pollution, reduces unnecessary material waste, reduces usage costs, and improves decolorization performance.
Smart Images

Figure CN118904318A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of decolorized sand, and in particular relates to an activation and regeneration method for decolorized sand. Background Art
[0002] Decolorizing sand refers to an adsorbent that uses decolorizing and filtering methods to absorb impurities and colors in regenerated oil. After being filtered through decolorizing sand, the oil becomes clear and bright, and the sulfide in the oil is removed, which improves the quality of the oil. It is the preferred decolorizing and adsorption product on the market.
[0003] In the related prior art, for example, a Chinese invention patent application discloses a method for activating and regenerating decolorized sand, with the publication number CN112090416A. The specific scheme disclosed in the patent is: "The activation and regeneration method comprises the following steps: A. taking the waste decolorized sand into a water pool, mixing and rinsing with deionized water, removing visible dirt on the surface of the waste decolorized sand, and removing floating oil and impurities on the surface of the water pool; B. discharging the sewage in the water pool of step A to the same height as the decolorized sand, adding an organic solvent for high-concentration mixing, and completing the mixing". The existing patent uses a demulsifier to demulsify the decolorized sand, followed by a subsequent treatment with an organic solvent; the regeneration process involves an organic solvent and a demulsifier, and the decolorization performance of the decolorized sand is still not ideal, and the reuse rate and utilization rate of the decolorized sand are low. Summary of the invention
[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a method for activating and regenerating decolorized sand, which has the characteristics of improving the reuse rate and utilization rate of waste decolorized sand.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A method for activating and regenerating decolorized sand, comprising the following activation and regeneration steps:
[0007] Step S1, weigh a certain amount of waste decolorized sand, put it into a large barrel container, then add a strong alkaline regeneration agent, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 4% to 5%, and then stir it evenly with a stirrer to obtain a mixture A;
[0008] Step 2 S2, then add a dilute acid regeneration agent to the mixture A, wherein the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration of 3% to 6%, wherein the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1: (0.8-1.5), and stir the mixture evenly with a stirrer again to obtain a mixture B;
[0009] Step 3 S3, add an appropriate amount of binder to the mixture B; then add deionized water at a ratio of 1:2, and add an oxidant with a volume concentration of 10%-30% and a flocculant with a volume concentration of 5%-20%, and stir evenly with a stirrer to obtain a mixture C, then let the mixture C stand for a time T1 of 1-5h, and use a heater to heat it with a heating temperature K set in the range of 110-240°C. During the heating process, the waste silica gel decolorization sand can be decomposed into a precipitate and a liquid layer, and then the decomposed liquid layer is filtered at least 3 times using a filter, and after the filtration is completed, the precipitate is filtered and dried using a sieve for standby use;
[0010] Step 4 S4: Place the filtered precipitate into a drying device for a drying time T2 of 1.5-3.5 hours, until the water in the precipitate is evaporated completely; activated and regenerated decolorized sand can be obtained.
[0011] As a preferred technical solution of the present invention, the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1:1.
[0012] As a preferred technical solution of the present invention, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 4.5%, and the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration of 3.7%.
[0013] As a preferred technical solution of the present invention, the adhesive is at least one of a polyurethane adhesive, a polyvinyl alcohol adhesive or a starch adhesive.
[0014] As a preferred technical solution of the present invention, when the adhesive is a starch adhesive, the raw material percentages of the starch adhesive are water 70-80%; starch 20-30%; caustic soda 2.4-2.8%; borax 2.7-3.2%; and formaldehyde 0.01-0.03%.
[0015] As a preferred technical solution of the present invention, the oxidant with a volume concentration of 10%-30% includes one of perchlorate, permanganate, dichromate or sodium peroxide.
[0016] As a preferred technical solution of the present invention, the flocculant with a volume concentration of 5%-20% includes one of polyaluminum chloride or polyaluminum sulfate or polyferric chloride or polyferric sulfate.
[0017] As a preferred technical solution of the present invention, a bleaching agent is added in step S3, and the bleaching agent includes any one of chlorine water, sodium peroxide or ozone.
[0018] As a preferred technical solution of the present invention, three filters with different filter mesh sizes are used in step S3;
[0019] The mesh number of the first filter for the first filtration is 120-160 meshes, the mesh number of the second filter for the second filtration is 180-200 meshes, and the mesh number of the third filter for the third filtration is 220-280 meshes.
[0020] As a preferred technical solution of the present invention, in step S3, the heating temperature K of the heater is set to 120° C., and in step S4, the drying time T2 of the drying equipment is set to 2 hours.
[0021] The present invention relates to an activation and regeneration method for decolorized sand, which has the following beneficial effects:
[0022] The activation and regeneration method of decolorized sand of the present invention uses waste decolorized sand as a basic raw material, adopts a potassium hydroxide regeneration agent with a concentration of 4% to 5%, a dilute hydrochloric acid regeneration agent with a concentration of 3% to 6%, and combines and adds a proper amount of adhesive to obtain activated and regenerated decolorized sand. The regenerated decolorized sand has better decolorization performance and has the characteristics of improving the reuse rate and utilization rate of the waste decolorized sand. It can not only save resources, but also reduce environmental pollution; at the same time, it avoids unnecessary material waste and reduces the use cost.
[0023] The present invention will be further described below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is an observation picture taken after waste diesel was treated with the decolorizing sand obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0025] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0026] Example 1
[0027] A method for activating and regenerating decolorized sand, the method comprising the following activation and regeneration steps:
[0028] Step S1, weigh a certain amount of waste decolorized sand, put it into a large barrel container, then add a strong alkaline regeneration agent, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 4%, and then stir it evenly with a stirrer to obtain a mixture A;
[0029] Step 2 S2, then adding a dilute acid regeneration agent to the mixture A, wherein the dilute acid regeneration agent is a 3% dilute hydrochloric acid regeneration agent, wherein the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1:0.8, and stirring again with a stirrer to obtain a mixture B;
[0030] Step 3 S3, add an appropriate amount of adhesive to the mixture B; then add deionized water at a ratio of 1:2, and add an oxidant with a volume concentration of 10%-30% and a flocculant with a volume concentration of 5%-20%, and stir evenly with a stirrer to obtain a mixture C, then let the mixture C stand for a time T1 (preferably 1-5h), T1 is selected as 2h, and a heater is used for heating, and the heating temperature K is set in the range of 110°C. During the heating process, the waste silica gel decolorization sand can be decomposed into a precipitate and a liquid layer, and then the decomposed liquid layer is filtered three times using a filter, and after the filtration is completed, the precipitate is filtered and dried using a sieve for standby use;
[0031] Step 4 S4: Place the filtered precipitate into a drying device for a drying time T2 of 1.5 h (preferably 1.5-3.5 h) until the water in the precipitate is evaporated completely; activated and regenerated decolorized sand can be obtained.
[0032] Other technical requirements for regeneration are: the filter is a 1000*2300*3.0 filter produced by Shenzhen Leijie Environmental Protection Technology Co., Ltd., and its main material is carbon steel, and the drying equipment is from Kunming Jinma Machinery Equipment Co., Ltd., which has double-sided circulation air transportation, vertical air transportation up and down, and a heat transfer area of 14 / square meter; in step S3, three filters with different filter mesh numbers are used; the first filter mesh number for the first filtration is 140 mesh (preferably 120-160 mesh), the second filter mesh number for the second filtration is 200 mesh (preferably 180-200 mesh), and the third filter mesh number for the third filtration is 260 mesh (preferably 220-280 mesh).
[0033] Example 2
[0034] A method for activating and regenerating decolorized sand, the method comprising the following activation and regeneration steps:
[0035] Step S1, weigh a certain amount of waste decolorized sand, put it into a large barrel container, then add a strong alkaline regeneration agent, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 4.15%, and then stir it evenly with a stirrer to obtain a mixture A;
[0036] Step 2 S2, then adding a dilute acid regeneration agent to the mixture A, wherein the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration of 3.1%, wherein the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1:0.9, and stirring again with a stirrer to obtain a mixture B;
[0037] Step 3 S3, add an appropriate amount of adhesive to the mixture B; then add deionized water at a ratio of 1:2, and add an oxidant with a volume concentration of 10%-30% and a flocculant with a volume concentration of 5%-20%, and stir evenly with a stirrer to obtain a mixture C, then let the mixture C stand for a time T1 (preferably 1-5h), T1 is selected as 2.5h, and a heater is used for heating, and the heating temperature K is set in the range of 115°C. During the heating process, the waste silica gel decolorization sand can be decomposed into a precipitate and a liquid layer, and then the decomposed liquid layer is filtered three times using a filter, and after the filtration is completed, the precipitate is filtered and dried using a sieve for standby use;
[0038] Step 4 S4: Place the filtered precipitate into a drying device for a drying time T2 of 2.5 h (preferably 1.5-3.5 h) until the water in the precipitate is evaporated completely; activated and regenerated decolorized sand can be obtained.
[0039] Other technical requirements for regeneration are: the filter is a 1000*2300*3.0 filter produced by Shenzhen Leijie Environmental Protection Technology Co., Ltd., and its main material is carbon steel, and the drying equipment is from Kunming Jinma Machinery Equipment Co., Ltd., which has double-sided circulation air transportation, vertical air transportation up and down, and a heat transfer area of 14 / square meter; in step S3, three filters with different filter mesh numbers are used; the first filter mesh number for the first filtration is 140 mesh (preferably 120-160 mesh), the second filter mesh number for the second filtration is 200 mesh (preferably 180-200 mesh), and the third filter mesh number for the third filtration is 260 mesh (preferably 220-280 mesh).
[0040] Example 3
[0041] A method for activating and regenerating decolorized sand, the method comprising the following activation and regeneration steps:
[0042] Step S1, weigh a certain amount of waste decolorized sand, put it into a large barrel container, then add a strong alkaline regeneration agent, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 4.5%, and then stir it evenly with a stirrer to obtain a mixture A;
[0043] Step 2 S2, then adding a dilute acid regeneration agent to the mixture A, wherein the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration of 3.7%, wherein the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1:1.0, and stirring again with a stirrer to obtain a mixture B;
[0044] Step 3 S3, add an appropriate amount of adhesive to the mixture B; then add deionized water at a ratio of 1:2, and add an oxidant with a volume concentration of 10%-30% and a flocculant with a volume concentration of 5%-20%, and stir evenly with a stirrer to obtain a mixture C, then let the mixture C stand for a time T1 (preferably 1-5h), T1 is selected as 3h, and a heater is used for heating, and the heating temperature K is set in the range of 120°C. During the heating process, the waste silica gel decolorization sand can be decomposed into a precipitate and a liquid layer, and then the decomposed liquid layer is filtered 4 times using a filter, and after the filtration is completed, the precipitate is filtered and dried using a sieve for standby use;
[0045] Step 4 S4: Place the filtered precipitate into a drying device for a drying time T2 of 3 hours (preferably 1.5-3.5 hours) until the water in the precipitate is completely evaporated; activated and regenerated decolorized sand can be obtained.
[0046] Other technical requirements for regeneration are: the filter is a 1000*2300*3.0 filter produced by Shenzhen Leijie Environmental Protection Technology Co., Ltd., and its main material is carbon steel, and the drying equipment is from Kunming Jinma Machinery Equipment Co., Ltd., which has double-sided circulation air transportation, vertical air transportation up and down, and a heat transfer area of 14 / square meter; in step S3, three filters with different filter mesh numbers are used; the first filter mesh number for the first filtration is 140 mesh (preferably 120-160 mesh), the second filter mesh number for the second filtration is 200 mesh (preferably 180-200 mesh), the third filter mesh number for the third filtration is 260 mesh (preferably 220-280 mesh), and the fourth filter mesh number for the fourth filtration is 260 mesh (preferably 220-280 mesh).
[0047] Example 4
[0048] A method for activating and regenerating decolorized sand, the method comprising the following activation and regeneration steps:
[0049] Step S1, weigh a certain amount of waste decolorized sand, put it into a large barrel container, then add a strong alkaline regeneration agent, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 5%, and then stir it evenly with a stirrer to obtain a mixture A;
[0050] Step 2 S2, then adding a dilute acid regeneration agent to the mixture A, wherein the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration of 6%, wherein the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1:1.5, and stirring again with a stirrer to obtain a mixture B;
[0051] Step 3 S3, add an appropriate amount of adhesive to the mixture B; then add deionized water at a ratio of 1:2, and add an oxidant with a volume concentration of 10%-30% and a flocculant with a volume concentration of 5%-20%, and stir evenly with a stirrer to obtain a mixture C, then let the mixture C stand for a time T1 (preferably 1-5h), T1 is selected as 5h, and a heater is used for heating, and the heating temperature K is set in the range of 200°C. During the heating process, the waste silica gel decolorization sand can be decomposed into a precipitate and a liquid layer, and then the decomposed liquid layer is filtered three times using a filter, and after the filtration is completed, the precipitate is filtered and dried using a sieve for standby use;
[0052] Step 4 S4: Place the filtered precipitate into a drying device for a drying time T2 of 3.5 h (preferably 1.5-3.5 h) until the water in the precipitate is evaporated completely; activated and regenerated decolorized sand can be obtained.
[0053] Other technical requirements for regeneration are: the filter is a 1000*2300*3.0 filter produced by Shenzhen Leijie Environmental Protection Technology Co., Ltd., and its main material is carbon steel, and the drying equipment is from Kunming Jinma Machinery Equipment Co., Ltd., which has double-sided circulation air transportation, vertical air transportation up and down, and a heat transfer area of 14 / square meter; in step S3, three filters with different filter mesh numbers are used; the first filter mesh number for the first filtration is 140 mesh (preferably 120-160 mesh), the second filter mesh number for the second filtration is 200 mesh (preferably 180-200 mesh), and the third filter mesh number for the third filtration is 260 mesh (preferably 220-280 mesh).
[0054] Comparative Example 1
[0055] The difference from Example 1 is that in step S1, no potassium hydroxide regeneration agent with a concentration of 4% is added, and other conditions remain the same as those of Example 1.
[0056] Comparative Example 2
[0057] The difference from Example 1 is that in step S2, no dilute hydrochloric acid regeneration agent with a concentration of 3% is added, and other conditions remain the same as those of Example 1.
[0058] Comparative Example 3
[0059] The difference from Example 1 is that: the potassium hydroxide regeneration agent with a concentration of 4% is not added in S1, and at the same time, the dilute hydrochloric acid regeneration agent with a concentration of 3% is not added in step S2, and the other conditions remain the same as those of Example 1.
[0060] Comparative Example 4
[0061] The difference from Example 1 is that no adhesive is added to S3, and other conditions remain the same as those of Example 1.
[0062] Comparative Example 5
[0063] The difference from Example 1 is that: no potassium hydroxide regeneration agent with a concentration of 4% is added in S1, and no dilute hydrochloric acid regeneration agent with a concentration of 3% is added in step S2, and no binder is added in S3. Other conditions remain the same as those of Example 1.
[0064] It should be noted that the adhesive in the above-mentioned embodiments 1-4 and comparative examples 1-5 of the present invention is at least one of polyurethane adhesive, polyvinyl alcohol adhesive or starch adhesive; when the adhesive is starch adhesive, the raw material percentage of the starch adhesive is 70-80% water; 20-30% starch; 2.4-2.8% caustic soda; 2.7-3.2% borax; 0.01-0.03% formaldehyde. The oxidant with a volume concentration of 10%-30% includes one of perchlorate, permanganate, dichromate or sodium peroxide. The flocculant with a volume concentration of 5%-20% includes one of polyaluminium chloride, polyaluminium sulfate, polyferric chloride or polyferric sulfate.
[0065] In order to make the color of the decolorized sand product obtained by the present invention whiter, a bleaching agent is added in step S3, and the bleaching agent includes any one of chlorine water, sodium peroxide or ozone. The bleaching effect of the bleaching agent is used to bleach the decolorized sand, so that the color of the decolorized sand product obtained is white, which is convenient for subsequent decolorization treatment.
[0066] Test process description and test results
[0067] Waste diesel with a chroma of 6.0 was selected and divided into 9 parts. The 9 parts of waste diesel were decolorized using the activated regenerated decolorizing sand obtained in Examples 1-4 of the present invention and the decolorizing sand obtained in Comparative Examples 1-5, respectively. The chroma and decolorization rate of the waste diesel in each case were recorded after the test. The test results are shown in Table 1.
[0068] Chromaticity value of waste diesel after decolorization Decolorization rate (%) Comparative Example 1 2.4 69 Comparative Example 2 2.8 71 Comparative Example 3 4.9 60 Comparative Example 4 3.2 72 Comparative Example 5 5.6 58 Example 1 1.5 90 Example 2 1.2 92 Example 3 0.5 98 Example 4 0.8 96
[0069] It can be seen from Table 1 above that the activated regenerated decolorizing sand obtained according to the present invention has a good decolorizing technical effect on waste diesel. It can be seen from the table that the decolorizing sand obtained in Example 3 has the best decolorizing effect.
[0070] Waste diesel with a chroma of 6.0 was selected and divided into 9 parts. The 9 parts of waste diesel were decolorized using the activated regenerated decolorizing sand obtained in Examples 1-4 of the present invention and the decolorizing sand obtained in Comparative Examples 1-5, respectively. Then, the decolorizing sand was filtered using the same filter as that used to make the decolorizing sand of the present invention. The filtered decolorizing sand was subjected to a cyclic decolorization treatment for multiple times according to the above operation, and the chroma and decolorization rate of the waste diesel in each case were recorded multiple times (taking 5 times as an example). The treatment results recorded for 5 cyclic decolorization treatments are shown in Table 2, and the treatment results recorded for 15 cyclic decolorization treatments are shown in Table 3.
[0071] Table 2 shows the processing results of Comparative Examples 1-5 and Examples 1-4:
[0072] Chromaticity value of waste diesel after decolorization Decolorization rate (%) Comparative Example 1 2.8 68 Comparative Example 2 3.5 66 Comparative Example 3 5.1 61 Comparative Example 4 3.8 69 Comparative Example 5 5.4 60 Example 1 1.8 90 Example 2 1.5 91 Example 3 0.6 97 Example 4 0.9 95
[0073] Table 3 shows the processing results of Comparative Examples 1-5 and Examples 1-4:
[0074] Chromaticity value of waste diesel after decolorization Decolorization rate (%) Comparative Example 1 3.6 67 Comparative Example 2 4.1 64 Comparative Example 3 5.2 59 Comparative Example 4 4.5 61 Comparative Example 5 5.9 55 Example 1 3.1 87 Example 2 2.4 89 Example 3 1.5 95 Example 4 1.9 93
[0075] From the above Table 2 and Table 3, we can see that: Figure 1 As shown, the decolorized sand obtained by the present invention still has good decolorization performance after being recycled for many times (5 times and 15 times of processing records), among which the decolorized sand obtained in Example 3 has the best decolorization performance; the reason should be that when the waste diesel oil passes through the sand layer of the decolorized sand of the present invention, the harmful impurities can be adsorbed on the surface of the decolorized sand particles, thereby effectively achieving the decolorization effect of the oil; therefore, the present invention uses waste decolorized sand as the basic raw material, adopts a potassium hydroxide regeneration agent with a concentration of 4% to 5%, a dilute hydrochloric acid regeneration agent with a concentration of 3% to 6%, and combines with the addition of an appropriate amount of adhesive to obtain activated and regenerated decolorized sand. The regenerated decolorized sand has better decolorization performance, and has the characteristics of being able to improve the reuse rate and utilization rate of the waste decolorized sand, which can not only save resources, but also reduce environmental pollution; at the same time, it avoids unnecessary material waste and reduces the cost of use.
[0076] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0077] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for activating and regenerating decolorized sand, It is characterized in that Includes the following activation and regeneration steps Step S1, weigh a certain amount of waste decolorized sand, put it into a large barrel container, then add a strong alkaline regeneration agent, the strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration of 4% to 5%, and then stir it evenly with a stirrer to obtain a mixture A; Step 2 S2, then add a dilute acid regeneration agent to the mixture A, wherein the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration of 3% to 6%, wherein the ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1: (0.8-1.5), and stir the mixture evenly with a stirrer again to obtain a mixture B; Step 3 S3, add an appropriate amount of binder to the mixture B; then add deionized water at a ratio of 1:2, and add an oxidant with a volume concentration of 10%-30% and a flocculant with a volume concentration of 5%-20%, and stir evenly with a stirrer to obtain a mixture C, then let the mixture C stand for a time T1 of 1-5h, and use a heater to heat it with a heating temperature K set in the range of 110-240°C. During the heating process, the waste silica gel decolorization sand can be decomposed into a precipitate and a liquid layer, and then the decomposed liquid layer is filtered at least 3 times using a filter, and after the filtration is completed, the precipitate is filtered and dried using a sieve for standby use; Step 4 S4: Place the filtered precipitate into a drying device for a drying time T2 of 1.5-3.5 hours, until the water in the precipitate is evaporated completely; activated and regenerated decolorized sand can be obtained.
2. The activation and regeneration method of decolorized sand according to claim 1, Features: The ratio of the dilute hydrochloric acid regeneration agent to the potassium hydroxide regeneration agent is 1:
1.
3. The activation and regeneration method of a decolorized sand as claimed in claim 1, Features: The strong alkaline regeneration agent is a potassium hydroxide regeneration agent with a concentration value of 4.5%, and the dilute acid regeneration agent is a dilute hydrochloric acid regeneration agent with a concentration value of 3.7%.
4. The activation and regeneration method of decolorized sand according to claim 1, Features: The adhesive is at least one of a polyurethane adhesive, a polyvinyl alcohol adhesive, or a starch adhesive.
5. The activation and regeneration method of decolorized sand according to claim 4, Features: When the adhesive is a starch adhesive, the raw material percentages of the starch adhesive are 70-80% water, 20-30% starch, 2.4-2.8% caustic soda, 2.7-3.2% borax, and 0.01-0.03% formaldehyde.
6. The activation and regeneration method of decolorized sand according to claim 1, Features: The oxidant with a volume concentration of 10%-30% includes one of perchlorate, permanganate, dichromate or sodium peroxide.
7. The activation and regeneration method of decolorized sand according to claim 1, Features: The flocculant with a volume concentration of 5%-20% includes one of polyaluminium chloride, polyaluminium sulfate, polyferric chloride or polyferric sulfate.
8. A method for activating and regenerating decolorized sand according to any one of claims 1 to 7, Features: In step S3, a bleaching agent is added, wherein the bleaching agent includes any one of chlorine water, sodium peroxide or ozone.
9. The activation and regeneration method of decolorized sand according to any one of claims 1 to 7, Features: In step S3, three filters with different filter mesh sizes are used; The mesh number of the first filter for the first filtration is 120-160 meshes, the mesh number of the second filter for the second filtration is 180-200 meshes, and the mesh number of the third filter for the third filtration is 220-280 meshes.
10. The activation and regeneration method for decolorized sand according to any one of claims 1 to 7, Features: In step S3, the heating temperature K of the heater is set to 120°C, and in step S4, the drying time T2 of the drying equipment is set to 2h.